EIT Agent
登录
← 校园网页目录

校园网页 · 学校官网

Effect of Ferroelectric Polarization on Ionic Transport and Resistance Degradation in BaTiO3 by PhaseField Approach

Effect of Ferroelectric Polarization on Ionic Transport and Resistance Degradation in BaTiO 3 by Phase-Field Approach Ye Cao, ‡,† Jie Shen, § Clive Randall, ‡ and Long-Qing Chen ‡ ‡Department of Materials Science and Engineering, The Pennsylvania State University, University Park, Pennsylvania 16802 §Department of Mathematics, Purdue University, West Lafayette, Indiana 47907 We proposed a model to study the resistance degradation behavior of ferroelectric oxides in the presence of ferroelectric spontaneous polarization by combining the phase-field model of ferroelectric domains and nonlinear diffusion equations for ionic/electronic transport. We took into account the nonperiod- ic boundary conditions for solving the electrochemical transport equations and Ginzburg –Landau equations using the Chebyshev collocation algorithm. We considered a single domain structure relative to a thin film BaTiO 3 single crystal orientated to the normal of the electrode plates (Ni) in a single parallel plate capacitor configuration. The capacitor was subjected to a dc bias of 0.5 V either along the polarization direction or opposite to the polarization direction at 25 °C. It is shown that the polarization bound charges at the metal/ferroelectric interface play an important role in charge carrier transport and leakage current evolution in BaTiO 3 capacitor. I. Introduction F ERROELECTRIC perovskites such as barium titanate (BaTiO3) have become essential materials in various electronic devices such as positive temperature resistors, tun- able microwave dielectrics, piezoelectric actuators/sensors, and multilayer ceramic capacitors (MLCCs). 1 Improving the reliability of ceramic capacitors emerges as a critical chal- lenge when operation continues under a continuous bias. Among all the factors affecting the reliability of MLCCs, the long-term resistance degradation is one of the most impor- tant. It is characterized by slowly increasing leakage currents under constant voltage stress, which eventually leads to the breakdown of the capacitors. Two major concerns about the resistance degradation phe- nomenon are: (1) What are the major reasons that result in the degradation and (2) What is the life time (reliability) of the capacitor. The first problem has been approached by a variety of experimental methods such as the impedance spec- troscopy (IS) and thermal simulated depolarization current (TSDC). 2–12 It is well recognized that the electromigration of oxygen vacancies toward cathode under dc bias is important to the resistance degradation, as is evidenced by the electro- coloration at the anode and cathode. 2,3 By using impedance spectroscopy (IS) and electron energy loss spectroscopy (EELS), Yang et al. 4 directly observed the oxygen vacancy segregation in BaTiO 3-based ceramic capacitor near the cath- ode, and oxygen vacancy pile-up at the cathode side within each grain. Yoon et al. 5–9 investigated the effect of acceptor (Mg) concentration on resistance degradation behavior in acceptor-doped BaTiO 3 ceramic capacitor. He pointed out that the increase in Mg concentration result in higher degra- dation rates due to the increase in oxygen vacancies. Liu et al. 10,11 carried out TSDC measurement on Fe-doped SrTiO3 single crystals and ceramics. It was found out that the TSDC peaks associated with the defect dipole, trapped charge, and oxygen vacancy motion are all influenced through degradation process. Liu also studied the charge car- riers in degraded SrTiO 3 using IS and EELS and suggested polaron conduction is induced at the cathode as a possible mechanism controlling the insulation transport process and ultimately describing the degradation behavior. 12 Despite all these investigations, however, due to the complexity of multi- ple factors influencing the degradation, such as acceptor dop- ing concentration, depolarization current, dielectric layer thickness, grain size, conductivity dependence on phase (fer- roelectric and paraelectric), nonlinear conduction, electrode roughness, and grain microstructure (grain size, core-shell microstructure), the interdependence and relative importance is not yet fully understood. In this investigation we theoretically address the degrada- tion kinetics in relation to ferroelectric phase and the role of spontaneous polarization. Typically there is an engineering approach to accessing statistical estimates of the failure times, and the data for this are collected through highly accelerated lifetime tests (HALTS). 13–15 This method access the time evolution of the electronic conduction under a dc voltage at various temperatures, and the long-term reliability is evaluated using the Eyring model. The testing is often done in the paraelectric phase, and estimated times for fail- ures are extrapolated into the ferroelectric phase which in reality is the operating condition of the capacitors. Such an assumption ignores the role of complex domain struc- tures, the associated electrostrictive and piezoelectric-induced strains that may have influence on the degradation kinetics. Lacking the ferroelectric contributions to the degradation mechanisms, the empirical extrapolations from HALTs mea- sured lifetimes in the paraelectric state may not be represen- tative of the ferroelectric-based capacitors working in their ferroelectric phases. On the other hand, mathematical models of ionic/electronic defect transport have been proposed to study current response and resistance degradation phenomenon. 16–27 Baiatu and Wa- ser et al. presented classic mathematic models in both SrTiO 3 single crystal and ceramics under high-field stress. 16,17 In these models the dielectric breakdown is mainly attributed to the electronic compensation for oxygen vacancies accumulation near cathode ( n /C25 2½V /C15/C15 O /C138 ; n and ½V/C15/C15 O /C138 are the electron and oxy- gen vacancy concentration.) Later Meyer et al. 18 suggested pinning of compensating electrons by the work function of the electrodes on both sides of Ba 0.3Sr0.7TiO3 thin film and did not observe any resistance degradation behavior. Strukov et al. 19 provided a model of coupled drift-diffusion equations for electrons and ions and examined the mobile ion distributions and current –voltage characteristics of thin film David Johnson—contributing editor Manuscript No. 34701. Received March 18, 2014; approved June 30, 2014. †Author to whom correspondence should be addressed. e-mail: yxc238@psu.edu 1 J. Am. Ceram. Soc., 1–8 (2014) DOI: 10.1111/jace.13162 © 2014 The American Ceramic Society Journal semiconductor memristive. However, these models do not take into account the effect of ferroelectric polarization on defect transport and current evolution. On the other hand, Xiao and Suryanarayana et al. proposed several models which incorporated the semiconducting properties of the wide band-gap ferroelectric perovskites by taking into account the interaction between space charges and polarization. 20–23 Most recently the charged domain walls are theoretically studied, and the electron and hole response to the polarization bound charge near the domain wall have been calculated. 24–27 Never- theless, these models are either limited to the equilibrium pro- files or subject to analytical approximation. In this work, we developed a phase-field model to study the resistance degradation phenomenon in the presence of ferroelectric polarization in ideal ferroelectric capacitor struc- tures. The phase-field approach has been extensively used to study the ferroelectric domain structures in both bulk sys- tems and thin films. 28–32 The phase-field simulation is based on the time-dependent Ginzburg –Laudau (TDGL) equation. We propose to solve the set of electrochemical transport equations using spectral method based on the Chebyshev transforms along the transport direction and Fourier trans- forms along the plane normal to the transport direction. They are discussed in Section III. II. Model In the phase-field simulation, we choose the spontaneous polarization Pi ¼ P1; P2; P3ðÞ as the order parameter to describe the domain structures in ferroelectrics. The total free energy of the system can be expressed as F ¼ Z V ½flanðPiÞþ fgradðPi;jÞþ felasðPi; eijÞþ felecðPi; EiÞ/C138 dV; (1) where V is the system volume and flan(Pi), fgrad(Pi,j), felas(Pi, ɛij), and felec(Pi, Ei) are the Landau –Devonshire free energy density, the gradient energy density, elastic energy density, and the electrostatic energy density, respectively. The Lan- dau–Devonshire free energy is written as a polynomial expansion of the polarization components P i. For an eighth- order expansion under mechanical stress-free boundary con- dition, it is 32 in which aij, aijk, and aijkl are the fourth, sixth, and eighth- order coefficients, respectively, and the second-order coefficient a1 is linearly proportional to temperature and obeys the Curie–Weiss law. The Landau coefficients and Curie tempera- ture Tc are here not considered in relation to oxygen stoichi- ometry.33 The gradient energy is introduced through the gradients of the polarization ( Pi,j = oPi/ oxj). For a general anisotropic system, the gradient energy density is calculated by fgradðPi;jÞ¼ 1 2 GijklPi;jPk;l; (3) in which Gijkl is the gradient energy coefficient. The elastic energy density felas is given by felas ¼ 1 2 Cijkleijekl ¼ 1 2 Cijklðeij /C0 e0 ijÞðekl /C0 e0 klÞ; (4) where Cijkl is the elastic stiffness tensor, e0 ij is the eigenstrain induced by the spontaneous polarization Pi (the eigenstrain induced by the defect segregation is currently not taken into consideration), and ɛij is the total strain of the bulk com- pared to the parent paraelectric phase. The elastic strain eij is calculated from eij ¼ eij /C0 e0 ij. Detailed calculation of the ei- genstrain and the total strain are described in reference [30]. To consider the dipole –dipole interaction during ferroelectric domain evolution, the electrostatic energy of a domain struc- ture is introduced through f elec ¼ fðEi; PiÞ¼/C0 1 2 e0erEiEj /C0 EiPi; (5) where Ei is the electric field component, ɛ0 and ɛr are the vacuum permittivity and dielectric constant of the material, respectively. Based on the Landau –Devonshire free energy density, the gradient energy density, elastic energy density, and the electro- static energy density calculated from Eqs. (2) to (5), the total free energy F is obtained from Eq. (1). The temporal evolution of order parameter P are governed by the TDGL equations oPiðx; tÞ ot ¼/C0 L dF dPiðx; tÞ ; i ¼ 1; 2; 3; (6) where L is the kinetic coefficient which is related to the domain movement and t is time. The local electric field in Eq. (5) is dependent on the space charges as well as the polarization-induced bound charges. It also depends on the boundary conditions on the film sur- faces. The local electric field/potential distribution is gov- erned by the Poisson equation /C0r 2w ¼ q /C0r/C15 Pi e0er ¼ q0ð2½V/C15/C15 O /C138þ p /C0 n /C0½ A0/C138Þ /C0 r /C15 Pi e0er ; (7) in which w is the local electric potential, q is the total space charge density, q0 is the unit charge, ½V/C15/C15 O /C138 ; n, p, and [ A 0 ] denote the local concentrations of oxygen vacancy, electron, hole, and ionized acceptor, respectively. The polarization- induced charges are introduced by /C0 ∇P. The electric field E * is related to the electric potential through E * ¼/C0 r w: (8) The boundary condition for the electric potential is defined as wjz¼0¼ Vað0Þ; wjz¼L¼ VaðLÞ; (9) in which Va(0) and Va(L) are specified from the externally applied potential bias at z = 0, L. flan ¼a1ðP2 1 þ P2 2 þ P2 3Þþ a11ðP4 1 þ P4 2 þ P4 3Þþ a12ðP2 1P2 2 þ P2 2P2 3 þ P2 3P2 1 Þ þ a111ðP6 1 þ P6 2 þ P6 3Þþ a112½P2 1ðP4 2 þ P4 3Þþ P2 2ðP4 1 þ P4 3Þþ P2 3ðP4 1 þ P4 2Þ/C138 þ a123P2 1P2 2 P2 3 þ a1111ðP8 1 þ P8 2 þ P8 3Þþ a1112½P6 1ðP2 2 þ P2 3Þþ P6 2ðP2 1 þ P2 3Þþ P6 3ðP2 1 þ P2 2Þ/C138 þ a1122ðP4 1P4 2 þ P4 2P4 3 þ P4 3P4 1 Þþ a1123ðP4 1P2 2 P2 3 þ P4 2P2 3 P2 1 þ P4 3P2 1 P2 2 Þ (2) 2 Journal of the American Ceramic Society—Cao et al. The bulk transports of space charges in Eq. (7) are described by the diffusion equations with proper boundary conditions. In our current simulation, the major charged defects of interest include the oxygen vacancies ( V /C15/C15 O ), elec- trons (e 0), holes ( h), ionized acceptors ( A0) written in Kr€oger–Vink notation. 34 The oxygen vacancies, electrons, and holes are considered as mobile species. The monovalent acceptors are introduced from the substitution of +3 elements such as Fe and Al on the Ti sites (Fe 0 Ti and Al 0 Ti ¼ A0) and are considered fully ionized and immobile. Due to extreme low mobility compared to electrons and holes, oxygen vacancies are considered to be the major fac- tors in determining the simulation time. The oxygen vacancy migration consists of the chemical diffusion due to concentra- tion gradient and the electrical drift under the external applied electric field. Here, we do not consider the presence of association and the formation of defect dipoles. A nonlin- ear Nernst –Planck transport model is applied to describe the oxygen vacancy migration, 35,36 in which ½V/C15/C15 O /C138 is the oxygen vacancy concentration, JV/C15/C15 O is the flux of the oxygen vacancy, DV/C15/C15 O and lV/C15/C15 O are the diffusiv- ity and mobility of oxygen vacancy, respectively, which are related with each other through the Nernst –Einstein equation DV/C15/C15 O ¼ kBT zV/C15/C15 O q0 lV/C15/C15 O ; (11) kB is the Boltzmann constant, T is the absolute temperature, zV/C15/C15 O ¼þ 2 denotes the charge number of oxygen vacancy, and q0 is the unit charge. Dφ12 and D x! are the electric potential difference and distance between two adjacent grid points, respectively. The Ni electrodes act as the blocking boundaries for oxy- gen vacancies migration during the resistance degradation so that the boundary condition for Eq. (10) can be written as JV/C15/C15 O /C12/C12/C12 z¼0;L ¼ 0: (12) On the other hand, electrons and holes are moving much faster than oxygen vacancies due to their higher mobility. In our simulations we assumed that the electron and hole con- centrations always reach equilibrium for each evolution of oxygen vacancy profile. Mathematically we solve steady-state equations for electron and hole transports assuming on/ ot = 0 and op/ot = 0 J n ¼/C0 Dnrn /C0 lnnE * on ot ¼/C0 r/C15 Jn ¼ Dnr2n þ lnr/C15 nE *hi ¼ 0 (13) Jp ¼/C0 Dprp þ lpnE * op ot ¼/C0 r/C15 Jp ¼ Dpr2p /C0 lpr/C15 pE *hi ¼ 0 : (14) The electron and hole concentrations at the Ni/BaTiO 3 interface are pinned by the Ni electrode as nz¼0;L ¼ Nc exp /C0 Ec /C0 Efm kBT /C18/C19 (15) pz¼0;L ¼ Nv exp /C0 Efm /C0 Ev kBT /C18/C19 ; (16) in which Nc and Nv are the effective density of states of the conduction band and valance band, respectively. Ec and Ev are the energy of the conduction band minimum and valence band maximum of BaTiO 3, respectively. Efm is the work function of Ni plate electrode. The current density is contributed from the flow of the charged species including oxygen vacancies, electrons, and holes. The current density for particular charged carrier i and the total current density are given by I i ¼ q0ziJi; i ¼ V/C15/C15 O ; e0; p/C15 (17) Itotal ¼ X i Ii; (18) in which zi and Ji denote the charge number and the flux of each of the charge species. III. Results and Discussions We first consider an ideal situation regarding the influence of a high spontaneous polarization on the transport processes. We consider a single tetragonal domain structure, such as a thin film BaTiO 3 single crystal orientated normal to the elec- trode plates (Ni) in a single parallel plate capacitor configu- ration. We set up a coordinate system with a periodic boundary condition along x and y directions. Along z direc- tion it is nonperiodic so that a Chebyshev collocation bound- ary condition is applied. We are mainly concerned with the ionic/electronic transport along z direction, and the polariza- tion direction is also assumed to be along z direction. There- fore, the system size of the simulation is chosen to be 1 9 1 9 200. The temporal evolution of the polarization field and thus the domain structures are obtained by numeri- cally solving the TDGL equations using the semi-implicit Fourier spectral method. 37–40 The corresponding material constants for the Landau free energy, the gradient energy coefficients, the electrostrictive coefficients, and elastic prop- erties are taken from the literature. 32,41 The parameters used in the simulation are listed in Table I. We started with a charge neutral single tetragonal domain BaTiO3 of thickness L = 500 nm constrained by Ni plate electrodes on two sides at room temperature (25 °C). The acceptor doping concentration was [ A 0 ] = 2.0 9 1018 cm/C0 3. All the ionic and electronic defects were assumed to be homogeneously distributed and the local charge neutrality condition was maintained in the initial state 2½V /C15/C15 O /C138þ p /C0 n /C0½ A0/C138¼ 0: (19) The initial polarization was assumed to be homogeneous and equal to the spontaneous polarization P = Ps = 26 lC/ JV/C15/C15 O ¼/C0 DV/C15/C15 O r½V/C15/C15 O /C138/C0 lV/C15/C15 O ½V/C15/C15 O /C138 2kBT zV/C15/C15 O q0D x! sinh zV/C15/C15 O q0D/12 2kBT /C18/C19 o½V/C15/C15 O /C138 ot ¼/C0 r/C15 JV/C15/C15 O ¼ DV/C15/C15 O r2½V/C15/C15 O /C138þ lV/C15/C15 O 2kBT zV/C15/C15 O q0D x! r½ V/C15/C15 O /C138 sinh zV/C15/C15 O q0D/12 2kBT /C18/C19/C18/C19 (10) Polarization Effect on Transport 3 cm2 which was oriented along the +z direction. The bound- ary condition of polarization at the metal/ferroelectric inter- face in 1D was specified as a /C2 P /C0 b /C2 dP dz /C12/C12/C12 /C12 z¼0 ¼ 0; a/C2 P þ b /C2 dP dz /C12/C12/C12 /C12 z¼L ¼ 0; (20) where coefficients a and b were chosen to be 1.0 and 0.05 cm, respectively, representing a partially compensated boundary condition. The simulation was then performed at T = 25°C until defect and polarization distributions reached steady state under no external bias, which are schematically plotted in Fig. 1(a). The equilibrium profiles are shown in Fig. 2. From Fig. 2(a) it is seen that the ferroelectric polarization remained constant inside the bulk BaTiO 3 and decreased at the metal/ ferroelectric interfaces. As a result, a sheet of positive bound charge was formed at one interface ( z/H =+ 1) and a nega- tive bound charge on the other ( z/H = /C0 1) [Fig. 2(b)]. For charge compensation, the positively charged oxygen vacan- cies and holes tended to segregate at z/H = /C0 1, while the negatively charged electrons at z/H =+ 1 [Figs. 2(c) and (d)]. It should be noted that the electronic concentrations are much lower than oxygen vacancies. This is because of the wide band gap ( ~3.1 eV) of BaTiO 3. 42 In response to the redistribution of polarization bound charges and the ionic/ electronic space charges, the local electric potential and elec- tric field were obtained from Eqs. (7) and (8) under the short circuit boundary condition V ajz¼/C0 H¼ Vajz¼H¼ 0 [Figs. 2(e) and (f)]. A large positive electric field was formed at the metal/ferroelectric interfaces due to electric potential to be 0 at the boundaries. When the equilibrium profile was reached, the resistance degradation simulations were carried out by applying a dc bias of 0.5 V along the polarization direction ( +z direction). Under the field stress, the oxygen vacancies were migrating toward the cathode side ( z/H =+ 1) [Fig. 3(a)], resulting in a positive ionic charge region at z/H =+ 1 and a negative ionic charge region at z/H = /C0 1, given that ionized acceptors are immobile. In response to the local ionic charges, the electrons (a) (b) (c) (d) Fig. 1. Schematic plot of the metal (Ni)/ferroelectric (BaTiO 3)/metal (Ni) sandwich structure: (a) without bias; (b) under applied bias in the same direction of polarization; (c) under applied bias in the reverse direction of polarization; (d) under applied bias without ferroelectric spontaneous polarization. The yellow and green arrows denote the directions of polarization and electric field, respectively. The ( +) and ( /C0 ) signs represent the anode and cathode, respectively. The and signs denote the polarization bound charge near the metal/ferroelectric interfaces. Table I. Parameters Used in the Simulation Parameter Value Temperature, T (K) 298 Total thickness, L (nm) 500 Dielectric constant, er 200 Electron/hole mobility, ln, lp [cm2 (V/C1 s)/C0 1] 0.67, 0.35 3 Oxygen vacancy mobility, lV/C15/C15 O [cm2 (V/C1 s)/C0 1] 1.0 9 10/C0 14 3 External bias (V) 0.5 Conduction band, Ec (eV) /C0 3.6 45 Valence band, Ev (eV) /C0 6.7 45 Work function of Ni electrode, Efm (eV) /C0 5.2 45 Effective density of states, Nc, Nv (cm/C0 3) 1022 (a) (d) (e) (f) (b) (c) Fig. 2. Equilibrium profile of single domain BaTiO 3 without bias: (a) polarization ( Pz), (b) polarization bound charge ( /C0 dPz/dz), (c) ionic defects (d) electronic defects, (e) electric potential, and (f) electric field ( z denotes the position in the film, H = 250 nm is half of the film thickness L, so that z/H from /C0 1t o +1 represents the entire thin film thickness). 4 Journal of the American Ceramic Society—Cao et al . tended to migrate toward the cathode and holes toward anode [Figs. 3(b) and (c)]. However, the electronic charge compensation was much smaller than the ionic charges since the electronic defects were pinned by the Ni plate electrodes at the boundaries. The electric potential evolution was plot- ted in Fig. 3(d), in which a large electric potential gradient was formed near the anode side in steady state. This agrees with recent experimental results by Okamoto et al. 43 in which a large electric field was observed at anode side in the degraded MLCCs. It should be noted that in the current sim- ulation we do not consider the possibility of anodic Ni plate electrode oxidation due to the oxygen vacancy depletion/ oxygen ion accumulation under long-term bias in the current simulation, which could change the capacitance value. We also applied a dc bias of 0.5 V in the opposite direc- tion of the polarization ( /C0 z direction). The reverse bias was small enough so that the single domain was not allowed to switch. For comparison we also considered the situation when there is no spontaneous polarization. Figures 1(b) –(d) schematically illustrates three different situations of BaTiO 3 single plate capacitor subject to dc biases. The oxygen vacancy evolutions were plotted in Figs. 4(a) –(c). In all three cases, the oxygen vacancies tended to migrate along the applied field direction. However, the oxygen vacancy (a) (b) (c) (d) Fig. 3. Defect transport and electric potential evolution in single domain BaTiO 3 plate capacitor at T = 25°C under dc bias (0.5 V) along +z direction (a) oxygen vacancies, (b) electrons, (c) holes, and (d) electric potential evolution. (a) (d) (e) (f) (b) (c) Fig. 4. Comparison of oxygen vacancy evolution (a –c) and local electric field (d –f) distribution in single crystal BaTiO 3 plate capacitor subjected to 0.5 V at T = 25°C (a) and (d): applied field in the same direction of polarization; (b) and (e): applied field in the opposite direction of polarization; (c) and (f): no polarization. Polarization Effect on Transport 5 segregation reached ~1020 cm/C0 3 along the cathode side when the field was along the polarization direction [Fig. 4(a)], it reached only ~2.5 9 10 19 cm/C0 3 when the field was opposite to the polarization direction [Fig. 4(b)] and ~4.4 9 1019 cm/C0 3 when there was no polarization [Fig. 4(c)]. A possible explanation for the difference is that the polarization pro- motes the ionic transport and further deteriorates the resis- tance of the capacitor when it is along the field direction. Note these concentrations are close to the Mott Criterion, and in the ferroelectric state are expected to be semiconduct- ing. 44 To further understand the differences of oxygen vacancy segregation among three situations, we investigated the electric field distribution inside the BaTiO 3 dielectric lay- ers [Figs. 4(d) –(f)]. From Fig. 2(f), positive electric fields were seen at Ni/BaTiO 3 interfaces without applied field. When a positive external bias was applied on BaTiO 3, the local fields at the boundaries was enhanced to 200 kV/cm [Fig. 4(d)], which acted as a large driving force for the oxy- gen vacancy migration along the +z direction. Under nega- tive bias, the field became negative inside the BaTiO 3 layer leading to the oxygen vacancies migration along /C0 z direc- tion. However, at the interfacial regions, the local field still remained positive ( ~50 kV/cm) at ~105 s [Fig. 4(e)], thus inhibited the further migration of oxygen vacancy toward cathode. When the ferroelectric polarization was zero, the local electric field at the interfaces reached ~120 kV/cm [Fig. 4(f)]. Therefore, the amount of oxygen vacancy segrega- tion with P = 0 lied between the other two cases. The current density evolutions were compared among the aforementioned three cases (Fig. 5). The leakage currents all experienced small and slow increases in the initial state when the oxygen vacancies started to migrate under the external biases, followed by fast and significant increases indicating the breakdown of the capacitor. The rapid leakage current increase could be attributed to the oxygen vacancy segrega- tion and the local field concentration in cathodes. The leakage current with P = 0 increased about one order of magnitude, and was remarkably enhanced ( ~409) under positive bias and inhibited ( ~59) under negative bias. This agrees with the evolution of oxygen vacancies and local fields shown in Fig. 4. It should also be noted that the current underwent an observable decrease before t = 10 5 s under negative bias (blue line in Fig. 5). This is because of the elec- tric current along +z direction due to the positive local field at cathode region [Fig. 4(e)], which offset the negative cur- rent along /C0 z direction inside the bulk BaTiO 3. When t > 105 s, the local field at cathode further decreased to nega- tive (blue line in Fig. 5) so that the total current along /C0 z direction increased. On the other hand, we also compared the mean time to failure (MTTF) among the three cases. The MTTF was determined as the leakage current increases one decade above its minimum value. From Figs. 4 and 5, it is evident that the ferroelectric polarization accelerates the oxy- gen vacancy migration, promotes the net leakage current increase and decreases the MTTF when it is along the applied field direction. The electric field dependence of MTTF was plotted for all three cases in Fig. 6(a). While the log(MTTF) versus log (field) curves exhibit almost linear relation at small field region, a nonlinear field dependence of MTTF is clearly seen at large field region for all the three cases [Fig. 6(a)]. This nonlinear dependence of current on electric field has been reported by Riess et al. 35,36 More recently, Randall et al. 15 suggested a ion conduction model to describe the transfer of oxygen vacancies and used it to account for MTTF data j ¼ 2q0Nav exp /C0 U kBT /C18/C19 sinh q0Ea 2kBT ; (21) in which j is the current, N is the number of ion, a is the dis- tance of ion hopping, v is the frequency of ion, U is the acti- vation energy dependent mainly on temperature, and E is the applied electric field strength. The life time of capacitor can Fig. 5. Leakage current evolution of BaTiO 3 single parallel layer capacitor under forward bias, reverse bias, and no polarization at 25°C. (a) (b) Fig. 6. Electric field strength dependence of mean time to failure of single plate BaTiO 3 capacitor (a) log tch versus log E, (b) log tch versus log sinh q0 Ea 2kB T /C16/C17 . 6 Journal of the American Ceramic Society—Cao et al . be considered as the time to a certain amount of transport charge accumulation ( Q), which is assumed to be constant at different temperature and voltage conditions. As a result, the MTTF can be represented as tch ¼ Q=j ¼ C exp /C0 U kBT /C18/C19 sinh q0Ea 2kBT /C18/C19 /C0 1 log tch ¼ C0 /C0 log sinh q0Ea 2kBT /C18/C19 : (22) A replot of the field dependence of MTTF with logtch ver- sus log sinh q0 Ea 2kB T /C16/C17 from our simulation clearly shows linear relations [Fig. 6(b)]. It is found out that the slopes of the curves are /C0 1.1, /C0 0.97, and /C0 0.97 for positive bias, negative bias, and no polarization cases, respectively. This agrees well with the phenomenological model proposed by Randall et al. 15 IV. Summary In this paper, we developed a phase-field model combined with nonlinear transport equations to study the resistance degradation behavior of mono-domain BaTiO 3 single plate capacitor. Our results show that the electrochemical migra- tion of oxygen vacancies contributes to the resistance degra- dation. On the other hand, the ferroelectric polarization modulates the local electric field distribution at the metal/fer- roelectric interfaces, promotes the oxygen vacancy segrega- tion and further deteriorates the resistance of the capacitor when it is along the direction of the external applied field. Our simulation result on the nonlinear electric field strength dependence of MTTF agrees well with a recently reported ion conduction model. In the future we will further extend the current model to incorporate the multidomain structures and grain structures to study their effect on transport dynam- ics and degradation behaviors. Acknowledgments The authors are grateful to the financial support by the NSF-IUCRC Center for Dielectric Studies at Penn State and the Air Force Office of Scientific Research under the Aerospace Materials for Extreme Environments Program. The work of Jie Shen is partially supported by NSF DMS-1215066 and by the Computational Materials and Chemical Sciences Network (CMCSN). References 1O. Auciello, J. F. Scott, and R. Ramesh, “The Physics of Ferroelectric Memories,” Phys. Today , 51 [7] 22 –7 (1998). 2R. Waser, T. Baiatu, and K. H. Hardtl, “Dc Electrical Degradation of Perovskite-Type Titanates .2. Single-Crystals,” J. Am. Ceram. Soc. , 73 [6] 1654–62 (1990). 3H. I. Yoo, M. W. Chang, T. S. Oh, C. E. Lee, and K. D. Becker, “Electro- coloration and Oxygen Vacancy Mobility of BaTiO3,” J. Appl. Phys. , 102, 093701, 8pp (2007). 4G. Y. Yang, G. D. Lian, E. C. Dickey, C. A. Randall, D. E. Barber, P. Pinceloup, M. A. Henderson, R. A. Hill, J. J. Beeson, and D. J. Skamser, “Oxygen Nonstoichiometry and Dielectric Evolution of BaTiO3. Part II — Insulation Resistance Degradation Under Applied dc Bias,” J. Appl. Phys. , 96 [12] 7500 –8 (2004). 5S. H. Yoon, M. H. Hong, J. O. Hong, Y. T. Kim, and K. H. Hur, “Effect of Acceptor (Mg) Concentration on the Electrical Resistance at Room and High (200 Degrees C) Temperatures of Acceptor (Mg)-Doped BaTiO3 Ceram- ics,” J. Appl. Phys. , 102, 054105, 9pp (2007). 6S. H. Yoon, C. A. Randall, and K. H. Hur, “Influence of Grain Size on Impedance Spectra and Resistance Degradation Behavior in Acceptor (Mg)- Doped BaTiO3 Ceramics,” J. Am. Ceram. Soc. , 92 [12] 2944 –52 (2009). 7S. H. Yoon, C. A. Randall, and K. H. Hur, “Effect of Acceptor (Mg) Con- centration on the Resistance Degradation Behavior in Acceptor (Mg)-Doped BaTiO3 Bulk Ceramics: II. Thermally Stimulated Depolarization Current Analysis,” J. Am. Ceram. Soc. , 92 [8] 1766 –72 (2009). 8S. H. Yoon, C. A. Randall, and K. H. Hur, “Correlation Between Resis- tance Degradation and Thermally Stimulated Depolarization Current in Acceptor (Mg)-Doped BaTiO3 Submicrometer Fine-Grain Ceramics,” J. Am. Ceram. Soc. , 93 [7] 1950 –6 (2010). 9S. H. Yoon, S. H. Kwon, and K. H. Hur, “Dielectric Relaxation Behavior of Acceptor (Mg)-Doped BaTiO(3),” J. Appl. Phys. , 109, 084117, 8pp (2011). 10W. Liu and C. A. Randall, “Thermally Stimulated Relaxation in Fe-Doped SrTiO3 Systems: I. Single Crystals,” J. Am. Ceram. Soc. , 91 [10] 3245–50 (2008). 11W. Liu, and C. A. Randall, “Thermally Stimulated Relaxation in Fe- Doped SrTiO3 Systems: II. Degradation of SrTiO3 Dielectrics,” J. Am. Ceram. Soc. , 91 [10] 3251 –7 (2008). 12W. Liu, G. Y. Yang, and C. A. Randall, “Evidence for Increased Polaron Conduction Near the Cathodic Interface in the Final Stages of Electrical Deg- radation in SrTiO(3) Crystals,” Jpn. J. Appl. Phys. , 48, 051404, 6pp (2009). 13R. Waser, T. Baiatu, and K. H. Hardtl, “Dc Electrical Degradation of Perovskite-Type Titanates .1. Ceramics,” J. Am. Ceram. Soc. , 73 [6] 1645 –53 (1990). 14S. Zhao, S. J. Zhang, W. Liu, N. J. Donnelly, Z. Xu, and C. A. Ran- dall, “Time Dependent dc Resistance Degradation in Lead-Based Perovsk- ites: 0.7 Pb(Mg(1/3)Nb(2/3))O(3)-0.3 PbTiO(3),” J. Appl. Phys. , 105, 053705, 7pp (2009). 15C. A. Randall, R. Maier, W. Qu, K. Kobayashi, K. Morita, Y. Miz- uno, N. Inoue, and T. Oguni, “Improved Reliability Predictions in High Permittivity Dielectric Oxide Capacitors Under High dc Electric Fields with Oxygen Vacancy Induced Electromigration,” J. Appl. Phys. , 113, 014101, 6pp (2013). 16T. Baiatu, R. Waser, and K. H. Hardtl, “Dc Electrical Degradation of Perovskite-Type Titanates .3. A Model of the Mechanism,” J. Am. Ceram. Soc., 73 [6] 1663 –73 (1990). 17T. Holbling, N. Soylemezoglu, and R. Waser, “A Mathematical-Physical Model for the Charge Transport in p-Type SrTiO3 Ceramics Under dc Load: Maxwell-Wagner Relaxation,” J. Electroceram. , 9 [2] 89 –102 (2002). 18R. Meyer, R. Liedtke, and R. Waser, “Oxygen Vacancy Migration and Time-Dependent Leakage Current Behavior of Ba0.3Sr0.7TiO3 Thin Films,” Appl. Phys. Lett. , 86, 112904, 3pp (2005). 19D. B. Strukov, J. L. Borghetti, and R. S. Williams, “Coupled Ionic and Electronic Transport Model of Thin-Film Semiconductor Memristive Behav- ior,” Small, 5 [9] 1058 –63 (2009). 20Y. Xiao and K. Bhattacharya, “Interaction of Oxygen Vacancies with Domain Walls and its Impact on Fatigue in Ferroelectric Thin Films,” vol. 5387, pp. 354 –65 in Proceedings Smart Structures and Materials 2004: Active Materials: Behavior and Mechanics , (2004). 21Y. Xiao, V. B. Shenoy, and K. Bhattacharya, “Depletion Layers and Domain Walls in Semiconducting Ferroelectric Thin Films,” Phys. Rev. Lett. , 95, 247603, 4pp (2005). 22Y. Xiao and K. Bhattacharya, “A Continuum Theory of Deformable, Semiconducting Ferroelectrics,” Arch. Ration. Mech. Anal. , 189 [1] 59 –95 (2008). 23P. Suryanarayana and K. Bhattacharya, “Evolution of Polarization and Space Charges in Semiconducting Ferroelectrics,” J. Appl. Phys. , 111, 034109, 11pp (2012). 24A. K. Tagantsev and G. Gerra, “Interface-Induced Phenomena in Polari- zation Response of Ferroelectric Thin Films,” J. Appl. Phys. , 100, 051607, 28pp (2006). 25M. Y. Gureev, A. K. Tagantsev, and N. Setter, “Head-to-Head and Tail- to-Tail 180 Degrees Domain Walls in an Isolated Ferroelectric,” Phys. Rev. B , 83, 184104, 18pp (2011). 26E. A. Eliseev, A. N. Morozovska, G. S. Svechnikov, V. Gopalan, and V. Y. Shur, “Static Conductivity of Charged Domain Walls in Uniaxial Ferro- electric Semiconductors,” Phys. Rev. B , 83, 235313, 8pp (2011). 27T. Sluka, A. K. Tagantsev, D. Damjanovic, M. Gureev, and N. Setter, “Enhanced Electromechanical Response of Ferroelectrics due to Charged Domain Walls,” Nat. Commun. , 3, 748, 7pp (2012). 28H. L. Hu, and L. Q. Chen, “Computer Simulation of 90 Degrees Ferro- electric Domain Formation in Two-Dimensions,” Mater. Sci. Eng. A Struct. Mater., 238 [1] 182 –91 (1997). 29Y. L. Li, S. Y. Hu, Z. K. Liu, and L. Q. Chen, “Phase-Field Model of Domain Structures in Ferroelectric Thin Films,” Appl. Phys. Lett. , 78 [24] 3878–80 (2001). 30Y. L. Li, S. Y. Hu, Z. K. Liu, and L. Q. Chen, “Effect of Substrate Con- straint on the Stability and Evolution of Ferroelectric Domain Structures in Thin Films,” Acta Mater. , 50 [2] 395 –411 (2002). 31Y. L. Li, L. Q. Chen, G. Asayama, D. G. Schlom, M. A. Zurbuchen, and S. K. Streiffer, “Ferroelectric Domain Structures in SrBi2Nb2O9 Epitaxial Thin Films: Electron Microscopy and Phase-Field Simulations,” J. Appl. Phys., 95 [11] 6332 –40 (2004). 32Y. L. Li, L. E. Cross, and L. Q. Chen, “A Phenomenological Thermody- namic Potential for BaTiO3 Single Crystals,” J. Appl. Phys. , 98, 064101, 4pp (2005). 33S. Lee, G. A. Rossetti, Z. K. Liu, and C. A. Randall, “Intrinsic Ferroelec- tric Properties of the Nonstoichiometric Perovskite Oxide Ba1-XTi1-yO3-x- 2y,” J. Appl. Phys. , 105, 093519, 6pp (2009). 34F. A. Kroger and H. J. Vink, “Relations Between the Concentrations of Imperfections in Crystalline Solids,” Solid State Phys. , 3, 307 –435 (1956). 35I. Riess and J. Maier, “Symmetrized General Hopping Current Equation,” Phys. Rev. Lett. , 100, 205901, 4pp (2008). 36I. Riess and J. Maier, “Current Equation for Hopping Ions on a Lattice Under High Driving Force and Nondilute Concentration,” J. Electrochem. Soc., 156 [1] P7 –20 (2009). 37Y. Cao, S. Bhattacharya, J. Shen, C. A. Randall, and L. Q. Chen, “Role of Polaron Hopping in Leakage Current Behavior of a SrTiO3 Single Crystal,” J. Appl. Phys. , 114, 224102, 7pp (2013). Polarization Effect on Transport 7 38L. Q. Chen and J. Shen, “Applications of Semi-Implicit Fourier-Spectral Method to Phase Field Equations,” Comput. Phys. Commun. , 108 [2–3] 147 –58 (1998). 39J. Shen and T. Tang, Spectral and High-Order Methods with Applications . Chinese Science Press, Beijing, China, 2006. 40J. Shen, T. Tang, and L. L. Wang, Spectral Methods: Algorithms, Analysis and Applications . Springer, Berlin, Germany, 2011. 41G. Sheng, J. X. Zhang, Y. L. Li, S. Choudhury, Q. X. Jia, Z. K. Liu, and L. Q. Chen, “Misfit Strain-Misfit Strain Diagram of Epitaxial BaTiO3 Thin Films: Thermodynamic Calculations and Phase-Field Simulations,” Appl. Phys. Lett. , 93, 232904, 3pp (2008). 42S. Lee, W. H. Woodford, and C. A. Randall, “Crystal and Defect Chemis- try Influences on Band Gap Trends in Alkaline Earth Perovskites,” Appl. Phys. Lett. , 92, 201909, 3pp (2008). 43T. Okamoto, S. Kitagawa, N. Inoue, and A. Ando, “Electric Field Con- centration in the Vicinity of the Interface Between Anode and Degraded Ba- TiO3-Based Ceramics in Multilayer Ceramic Capacitor,” Appl. Phys. Lett. , 98, 072905, 3pp (2011). 44S. Lee, J. A. Bock, S. Trolier-McKinstry, and C. A. Randall, “Ferroelec- tric-Thermoelectricity and Mott Transition of Ferroelectric Oxides with High Electronic Conductivity,” J. Eur. Ceram. Soc. , 32 [16] 3971 –88 (2012). 45J. F. Scott, Ferroelectric Memories . Springer, Berlin, Germany, 2000. h 8 Journal of the American Ceramic Society—Cao et al .

采集于

查看校方原文 ↗