EIT Agent
登录
← 校园网页目录

校园网页 · 学校官网

Role of polaron hopping in leakage current behavior of a SrTiO3 single crystal.pdf

Role of polaron hopping in leakage current behavior of a SrTiO3 single crystal Y. Cao, S. Bhattacharya, J. Shen, C. A. Randall, and L. Q. Chen Citation: Journal of Applied Physics 114, 224102 (2013); doi: 10.1063/1.4842836 View online: http://dx.doi.org/10.1063/1.4842836 View Table of Contents: http://scitation.aip.org/content/aip/journal/jap/114/22?ver=pdfcov Published by the AIP Publishing [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27 Role of polaron hopping in leakage current behavior of a SrTiO 3 single crystal Y . Cao,1,a) S. Bhattacharya,2 J. Shen,3 C. A. Randall,1 and L. Q. Chen 1 1Department of Materials Science and Engineering, Penn State University, University Park, Pennsylvania 16802, USA 2Department of Materials Science and Engineering, Indian Institute of Technology Hyderabad, YM 502205, India 3Department of Mathematics, Purdue University, West Lafayette, Indiana 47907, USA (Received 4 September 2013; accepted 22 November 2013; published online 10 December 2013) We studied the ionic/electronic transport and resistance degradation behavior of dielectric oxides by solving the electrochemical transport equations. Here, we took into account the non-periodical boundary conditions for the transport equations using the Chebyshev collocation algorithm. A sandwiched Ni jSrTiO 3jNi capacitor is considered as an example under the condition of 1.0 V, 1.0 lm thickness for SrTiO 3 layer, and a temperature of 150 /C14 C. The applied voltage resulted in the migration of ionic defects (oxygen vacancies) from anode towards cathode. The simulated electric potential profile at steady state is in good agreement with the recent experimental observation. We introduced the possibility of polaron-hopping between Ti 3þ and Ti 4þ at the electrode interface. It is shown that both the oxygen vacancy transport and the polaron-hopping contribute to the resistance degradation of single crystal SrTiO 3, which is consistent with the experimental observations. VC 2013 AIP Publishing LLC .[ http://dx.doi.org/10.1063/1.4842836] I. INTRODUCTION Dielectric and ferroelectric perovskites, such as lead- zirconate titanite (PZT), strontium titanite (SrTiO 3), and bar- ium titanite (BaTiO 3), have been widely utilized in various electronic devices such as sensors, actuators, varistors, and multilayer ceramic capacitors (MLCCs). 1 High density inte- gration of devices and the desire for larger capacitance require ever-decreasing physical size and thickness for the dielectric layers. As a result, the reliability of these devices at reduced sizes, higher fields, and operating temperatures has become a major concern in capacitor industry. Among all the factors that affect the lifetime of MLCCs, the long-term resistance degradation emerged as one of the most important. It is characterized by slowly increasing leakage currents under dc field stress, followed by a rapid increase of currents indicating the breakdown of capacitors (Fig. 1). Experimentally, the highly accelerated lifetime test- ing (HALT) has been most widely used to investigate the degradation phenomenon in dielectric and ferroelectric perovskites. 2,3 It is well recognized that electrotransport of oxygen vacancies plays an important role in the resistance degrada- tion, as is evidenced by the electrocoloration at the anode and cathode. 4,5 However, the role of oxygen vacancy migra- tion in degradation is still not clear. Using High Resolution Transmission Electron Microscopy (HRTEM) and Electron Energy Loss Spectroscopy (EELS), Yang et al. examined the oxygen vacancy distribution after degradation and observed an increase of oxygen vacancy across the dielectric layers towards the cathode. Within each BaTiO 3 grain, there was a pileup of oxygen vacancies in the cathodic side and a net decrease towards the anodic side of the grain due to the blocking effects of grain boundaries. 6 Yoon et al. suggested that the increase of effective acceptor concentration (Mg) of BaTiO 3 as the grain size decreases causes high oxygen va- cancy concentrations, leading to faster degradation rates. 7 Yoon also found out that the space charge polarization at grain boundaries by the charge carriers of pre-dominant holes and small portion of oxygen vacancies results in dielectric relaxation in BaTiO 3.8 Despite all these works, however, due to the complexity that many factors may influ- ence the degradation, such as acceptor doping, polarization current, dielectric layer thickness, and electrode microstruc- ture, the key mechanism of resistance degradation has not yet been well understood experimentally. On the other hand, mathematical models of ionic/elec- tronic defect transport have been proposed to study current response and resistance degradation phenomenon. 9–13 Baiatu and Waser et al. presented mathematic models for SrTiO 3 single crystals and ceramics under high electric field stress.9,10 In these models, the dielectric breakdowns were mainly attributed to the electronic compensation for oxygen vacancies accumulated near cathode ( n /C25 2½V •• O /C138 ). Later, Meyer et al. suggested pinning of compensating electrons by the work function of the electrodes on both sides of Ba 0.3Sr0.7TiO3 thin film but did not observe any resistance FIG. 1. Schematic plot of a typical time dependent leakage current evolution during a HALTs test.a)Electronic mail: yxc238@psu.edu 0021-8979/2013/114(22)/224102/7/$30.00 VC 2013 AIP Publishing LLC114, 224102-1 JOURNAL OF APPLIED PHYSICS 114, 224102 (2013) [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27 degradation behavior. 11 More recently, a new mean time to failure (MTTF) equation was introduced by Randall et al. that considered critical accumulation of oxygen vacancies concentration under different field and temperatures to more accurately predict the degradation rates. 12 Strukov et al. pro- vided a model of coupled drift-diffusion equations for elec- trons and ions and examined the mobile ion distributions and current–voltage characteristics of thin film semiconductor memristor. 13 With all of this interest in coupled electronic and ionic conduction in mixed oxide functional materials, there is a need for deeper understanding of the transient proc- esses that occur on a local and macroscopic scale in these materials. The main objective of this work is to explore the contri- bution of polaron hopping conduction 14 between Ti 3þ and Ti4þ to the mechanism of resistance degradation that occurs in high concentrations of oxygen vacancies. We propose to solve the set of electrochemical transport equations using spectral method based on Chebyshev transforms along the transport direction and Fourier transforms along the plane normal to the transport direction. II. MODEL We chose acceptor doped SrTiO 3 single crystal as an example and studied the resistance degradation mechanism. The SrTiO3 thin film was constrained on both sides by the Ni electrodes. The major defects of interest included the oxygen vacancies ( V •• O ), electrons ( e0), holes ( h•), polarons, and ion- ized acceptors ( A0). The oxygen vacancies, electrons, holes, and polarons were considered as mobile species, while the ionized acceptors were assumed to be immobile. The mono- valent acceptors were introduced from the substitution of þ3 elements such as Fe and Al on the Ti sites (Fe 0 Ti and Al0 Ti¼ A0). The reduction-oxidation reaction and the intrinsic electron-hole generation in Kr €oger-Vink notation were con- sidered as major defect reactions in the current study. They are listed in Eqs. (1) and (2) with corresponding reaction constants collected from literature 9 OO ¼ 1 2 O2ðgÞþ V•• O þ 2e0; (1a) KO ¼½ V•• O /C138 n2p1=2 O2 ¼ 1:4 /C2 1071exp /C0 5:18 eV kBT /C18/C19 cm/C0 9Pa1=2; (1b) nil ¼ e0 þ h•; (2a) Ki ¼ np ¼ NcNv exp /C0 Eg kBT /C18/C19 cm/C0 6; (2b) in which KO and Ki are the chemical reaction constants, pO2 is the oxygen vacancy partial pressure, Nc and Nv are the effective density of states of the conduction and valance bands in the thin film, respectively, and Eg is the band gap of single crystal SrTiO 3. Due to extremely low mobility of oxygen vacancies compared to electrons and holes, they are considered to be the major factor in determining the long time dependent evo- lution. The oxygen vacancy migration consists of the chemi- cal diffusion due to concentration gradient and the electrical drift under an electric field. A classic Nernst-Planck transport model has been applied to describe the oxygen vacancies migration J V•• O ¼/C0 DV•• O r½V•• O /C138þ lV•• O ½V•• O /C138 E * ; @½V•• O /C138 @t ¼/C0 r •JV•• O ; (3) in which ½V•• O /C138 is the oxygen vacancy concentration, JV•• O is the flux of the oxygen vacancy, DV•• O and lV•• O are the diffusiv- ity and mobility of oxygen vacancy, respectively, which are related to each other through the Nernst-Einstein equation, D V•• O ¼ð kBT=zV•• O e0ÞlV•• O , in which kB is the Boltzmann con- stant, T is the absolute temperature, zV•• O ¼þ 2 denotes the effective valence for oxygen vacancy, and e0 is the unit charge. The Ni electrodes act as the blocking boundaries for oxygen vacancies during the resistance degradation such that the boundary condition for Eq. (3) can be written as JV•• O jz¼0;L ¼ 0: (4) E * in Eq. (3) is the local electric field dependent on the charged carrier distribution. It also depends on the boundary conditions on the film surfaces. The local electric field/ potential distribution is described by the Poisson equation /C0r 2w ¼ q e0er ¼ eð2½V•• O /C138þ p /C0 n /C0 npolaron /C0½ A0/C138Þ e0er ; (5) in which w is the local electric potential, q is the total defect charge distribution, ½V•• O /C138 , n, p, npolaron ,a n d ½A0/C138 denote the local concentration of oxygen vacancy, electron, hole, po- laron, and ionized acceptors, respectively. The electric poten- tial w is related to the electric field through E * ¼/C0 r w. The boundary condition for the electric potential is defined as wjz¼0 ¼ Vað0Þþ g; wjz¼L ¼ VaðLÞ/C0 g; (6) in which Vað0Þ and VaðLÞ are the applied potential bias at z ¼ 0; L. g is the overpotential of the electrochemical reac- tion occurred at the metal/semiconductor interface. On the other hand, electrons and holes are moving much faster than oxygen vacancies due to their higher mobility. In our simulation, we assume that the electronic species always reach equilibrium for each concentration evolution of oxy- gen vacancy profile. The transport of electrons and holes are described in the following equations: J n ¼/C0 Dnrn /C0 lnnE * ; @n @t ¼/C0 r •Jn ¼ Dnr2n þ lnr•½nE * /C138¼ 0; (7) Jp ¼/C0 Dprp þ lppE * ; @p @t ¼/C0 r •Jp ¼ Dpr2p /C0 lpr•½pE * /C138¼ 0: (8) 224102-2 Cao et al. J. Appl. Phys. 114, 224102 (2013) [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27 The electron and hole concentrations at the Ni/SrTiO 3 inter- face are pinned by the Ni electrode as nz¼0;L ¼ Nc exp /C0 Ec /C0 Efm kBT /C18/C19 ; (9) pz¼0;L ¼ NV exp /C0 Efm /C0 Ev kBT /C18/C19 : (10) The energy of the conduction band ( Ec) and valence band (Ev) and the work function of the metal electrode ( Efm ) are listed in Table I. We proposed a polaron hopping conduction model to study its effect on the leakage current evolution. The polar- ons were treated as localized monovalent charge carriers and they contribute to the total current by hopping between Ti 3þ and Ti 4þ sites, i.e., Ti4þ þ e/C0 ¼ Ti3þ. A schematic plot of the polaron hopping model is shown in Fig. 2. The flux of polarons at the cathode ( Ti4þ þ e/C0 ¼ Ti3þ) is described by the so called Butler-Volmer equation Jcathode ¼ Jf ðcathodeÞ /C0 JbðcathodeÞ ¼ kþcTi4 þ exp ð1 /C0 bÞnF RT g /C20/C21 /C0 k/C0 cTi3 þ exp /C0 bnF RT g /C20/C21 ; (11) in which cTi4 þ and cTi3 þ are the local concentration of Ti 4þ and Ti 3þ, respectively, kþ and k/C0 are the forward and back- ward reaction rate constants, b is the transfer coefficient, and g is the overpotential of the reaction. Similarly, the flux of polaron at the anode ( Ti3þ ¼ Ti4þ þ e/C0 ) is written as Janode ¼ Jf ðanodeÞ /C0 JbðanodeÞ ¼ kþcTi3 þ exp /C0 bnF RT g /C20/C21 /C0 k/C0 cTi4 þ exp ð1 /C0 bÞnF RT g /C20/C21 : (12) The electrotransport of polarons follows a diffusion equation with the boundary conditions determined by the flux which is given in Eqs. (11) and (12). The current density is determined from the flow of the charged species of oxygen vacancies, electrons, holes, and polarons. Ionized acceptors are assumed to be immobile so that they do not contribute to the current density. The current density for particular charged carrier i and the total current density are given by I i ¼ e0ziJi; (13) Itotal ¼ X i Ii; (14) in which i denote oxygen vacancy, electron, hole, or polaron. III. RESULTS AND DISCUSSION We considered SrTiO 3 single crystal as an example rela- tive to a single dielectric layer oriented to the normal of the electrode plates. We set up a coordinate system with periodic boundary condition along x and y directions. Along z direc- tion, it is non-periodic so that a Chebyshev collocation boundary condition was applied. Initially, we were mainly concerned with the ionic/electronic transport along z direc- tion. Therefore, the system size of the simulation was chosen to be 1 /C2 1 /C2 200. To solve the above equations, the semi-implicit Fourier- spectral method was employed. 15 Considering the time de- pendent transport [Eq. (3)], more generally, we rewrite it as @Cðr; tÞ @t ¼ Dr2Cðr; tÞ/C0 lr•½Cðr; tÞE * /C138 ; (15) in which Cðr; tÞ is the concentration of the diffusant and the diffusivity D is assumed to be space independent. Solving the above equation with a finite difference or Fourier approx- imation in space has a severe time step limit of Dt /C20 k=N 2 where k is a constant and N is the number of lattice points in each space dimension. To avoid this limitation, a semi- implicit treatment is considered. From Eq. (15), we have Cnþ1 /C0 Cn Dt ¼ Dr2Cnþ1 /C0 lr•½CnE * /C138 ; Cnþ1 DDt /C0r 2Cnþ1 ¼ Cn DDt /C0 l D /C18/C19 r•½CnE * /C138 ; (16) write u ¼ Cnþ1, a ¼ 1=ðDDtÞ,a n d f ¼ Cn=ðDDtÞ /C0 l=DðÞ r •½CnE * /C138 ,E q .(16) can be simplified as au /C0r 2u ¼ f ; (17) with periodic boundary condition along x and y directions and a non-periodic boundary condition along z direction. At TABLE I. Parameters for the simulation. Parameter Value Parameter Value pO2 0.1 Pa ½A0/C138 2.0 /C2 1018 cm/C0 3 EC /C0 4.0 eV lV•• O 1.0 /C2 10/C0 9cm2/C1 V/C0 1/C1 s/C0 1 EV /C0 7.0 eV ln 1.6 cm2/C1 V/C0 1/C1 s/C0 1 Eg 3.0 eV lp 0.8 cm2/C1 V/C0 1/C1 s/C0 1 Efm /C0 5.3 eV lpolaron 0.01 cm2/C1 V/C0 1/C1 s/C0 1 L 1.0 lm b 0.5 er 150 g 0.1 V FIG. 2. Schematic plot of the Ni|SrTiO 3|Ni sandwich structure and the small polaron hopping between Ti 3þ and Ti4þ (Ti4þ þ e/C0 ¼ Ti3þ). 224102-3 Cao et al. J. Appl. Phys. 114, 224102 (2013) [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27 each time step, Eq. (17) can be accurately solved using Chebyshev collocation algorithm. Details of this algorithm are described in the Appendix. We started with a charge neutral single crystal SrTiO 3 with film thickness L ¼ 1 lm of acceptor doping concentra- tion ½A0/C138¼ 2:0 /C2 1018cm/C0 3. The simulation condition and the parameters of the material are listed in Table I. We first performed the simulation of charge transport without taking into account the polaron hopping conduction. The initial charged defect concentrations were assumed to be homoge- neous and calculated based on the defect chemical reaction (Eqs. (1) and (2)) and the local neutrality condition, with monovalent acceptors mainly compensated by the oxygen vacancies 2½V •• O /C138þ p /C0 n /C0½ A0/C138¼ 0: (18) The simulation was then performed at T ¼ 1000 K with pO2 ¼ 0:1Pa to simulate the annealing process of the sample with Ni electrodes at elevated temperature. The oxygen va- cancy concentrations at the metal/dielectric interfaces were determined from Eq. (1b) ½V•• O /C138j z¼0;L ¼ KO n2 z¼0:Lp1=2 O2 ; (19) in which nz¼0:L is the electron concentration at the interface which is assumed to be pinned by the work function of metal electrodes (Eqs. (9) and (10)). By numerically solving the coupled equations (Eqs. (3), (5), (7), and (8)) with appropri- ate boundary conditions (Eqs. (6), (9), (10), and (19)), we obtained the equilibrium profiles of space charges and inte- rior electric potential for the initial unbiased condition as shown in Fig. 3. From Fig. 3(a), it can be seen that the thin film remained charge neutral. In the vicinity of the Ni/SrTiO 3 interfaces, however, negatively charged layers were formed with enrichment of electrons and depletion of oxygen vacancies and holes. An upward bending electric potential profile was formed in response to the ionic and electronic redistribution (Fig. 3(b)). After the charged defects and electric potential distribu- tion reached equilibrium, the resistance degradation simula- tion was implemented by applying an external potential bias of 1.0 V on the sample at T ¼ 150 /C14 C. At low temperature, the Ni electrodes acted as blocking boundaries for oxygen vacan- cies transport (Eq. (4)) so that the total oxygen vacancies remained constant. Electron and hole concentrations at the interfaces were still pinned by the Ni electrodes (Eqs. (9) and (10)). Fig. 4 shows the evolution profiles of charged defects and electric potential, with cathode on the left side ( z ¼ 0, w ¼ 0) and anode on the right hand side ( z ¼ L,w ¼ 1:0V). In Fig. 4(a), the oxygen vacancies tended to migrate towards the cathode under the electric field, resulting in a net positive charge layer near cathode and negative charge layer near an- ode. On the other hand, electrons and holes tended to redis- tribute to compensate the net charges induced from oxygen vacancy segregation and depletion (Figs. 4(b) and 4(c)). It should be noted that the electronic charge compensation was limited based on the assumption that electronic defect concentrations at the metal/dielectric interfaces were pinned by the work function of the metal electrodes. The electric potential distribution at steady state was almost constant inside the thin film and near cathode region due to charge screening. However, it exhibited a large gradient near anode side, indicating a locally concentrated electric field along – z direction (Fig. 4(d)). This is due to the ionic depletion in the vicinity of the anode. Our simulation result is consistent with recent experimental work by Okamoto et al. in which a highly concentrated electric field along anode side was observed in the degraded MLCCs. 16 The leakage current evolution under an electric field was studied and plotted in Fig. 5. It is seen that the current density experienced a small increase in the initial stage (t < 10 s) until it reached constant and no longer changed with time. The net current density increase was below one order of magnitude and thus there was no resistance degradation phenomenon in single crystal SrTiO 3 under the current simulation condition. In our current model, we pinned the boundary concentrations of electronic defects based on the Fermi level of the metallic electrode, and thus limited the electronic contribution to the leakage current. Our result showing no degradation in acceptor doped SrTiO 3 single crystal is different from what was previously reported, 9 that the current density increased FIG. 3. The ionic/electronic charged defects and inner potential distribution in equilibrium SrTiO 3 single layer of 1 lm in thickness at T ¼ 1000 K (with no external applied potential bias). (a) oxygen vacancy, electron, hole, and fully ionized acceptors; (b) inner potential profile. 224102-4 Cao et al. J. Appl. Phys. 114, 224102 (2013) [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27 by at least one order of magnitude due to the dramatic increase in the electron concentration near the cathode, /C24 10 18 cm/C0 3, to compensate the segregated oxygen vacancy in that region. However, our result agrees with more recent work on dc current response of a Ba 0.3Sr0.7TiO3 thin film ca- pacitor by Meyer et al. ,11 who showed that there was no re- sistance degradation also based on the assumption that the electron concentration at the electrode/dielectric interfaces is pinned by the electrodes. The fact that real dielectric capacitors’ display degrada- tion indicates that there must be other aspects to the total degradation mechanism. Recently, a small polaron hopping conduction was suggested as a possible mechanism for the dielectric degradation phenomenon. 14 The main objective of this work is to test the hypothesis that polaron hopping makes important contribution to the leakage current evolu- tion. The temporal profiles of polaron evolution were obtained by solving the diffusion equation using boundary conditions (11) and (12). The initial polaron concentration in SrTiO 3 was estimated to be 10 14 cm/C0 3 based on literature. 17 From Fig. 6, the polaron concentration started to increase at the cathode side, due to a net flow of electrons from cathode into the dielectric layer. The polaron concentration reached /C24 1017 cm/C0 3 in compensation to the excess of positive charges due to the oxygen vacancy segregation at the cath- ode side (Fig. 4(a)). In the anode region, the polaron concen- tration decreased for charge balance due to the significant oxygen vacancy depletion in the anode region (Fig. 4(a)). Our simulation result was evidenced by the recent experi- ment, in which a high local polaron concentration was observed in the degraded cathode region of a 1% Fe-doped FIG. 4. Evolution of charged defects and electric potential profile to steady state for SrTiO 3 at T ¼ 150 /C14 C under a 1.0 V external bias (a) oxygen vacancy; (b) electron; (c) hole, and (d) electric potential profile. FIG. 5. Calculated time-dependent leakage current evolution under 1.0 V dc bias at 150 /C14 C. 224102-5 Cao et al. J. Appl. Phys. 114, 224102 (2013) [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27 single crystal SrTiO 3.14 The simulated polaron concentration in cathode was two orders of magnitude lower than that in paper of Liu et al.14 This is because of a much higher doping concentration ( /C24 1%) in their experiments, which result in the oxygen vacancy accumulation up to 10 20 cm/C0 3. The current density evolution, which takes into account the polaron hopping conduction, is shown in Fig. 7. The leak- age current density remained low in the initial time range (<10 s) and increased significantly at /C24 10 s, when oxygen vacancies, free electrons, and polarons tended to segregate at the cathode side. As pointed out by Meyer et al., 11 the trans- port of oxygen vacancies and the ionic conduction itself does not fully explain the degradation process. Based on our simu- lation, the increase of ionic current was limited (Fig. 5), and the contribution of free electronic electrons to the leakage current was negligible due to extreme low electronic concen- tration, the leakage current increase by more than one order of magnitude could be explained by the local polaron hop- ping conduction. This was further evidenced by the correla- tion between the polaron concentration in cathode and leakage current density in the process of resistance degrada- tion. It is seen from Fig. 8 that the calculated polaron concentration increased with the degree of degradation. This agrees with Liu’s experimental results. 14 Therefore, it can be suggested that the polaron hopping conduction should be con- sidered as a possible mechanism for the resistance degrada- tion behavior in single crystal SrTiO 3 and other dielectrics. IV . SUMMARY In this paper, we studied the resistance degradation behavior of acceptor doped SrTiO 3 single crystal by solving the coupled defect transport and Poisson equations using Chebyshev Collocation Algorithm. Our simulation success- fully showed the ionic and electronic transport under exter- nal field and the steady state profile of electric potential, which is consistent with the recent experimental result. Our simulation showed no resistance degradation behavior based on the assumption that the electronic defects are pinned by the work function of metal electrodes at the interfaces. This agrees with the recent work by Meyer et al. Finally, by intro- ducing the polaron hopping between Ti 3þ and Ti 4þ into the current model, we successfully modeled leakage current behavior and suggest that the resistance degradation phe- nomenon in dielectric capacitors can possibly be explained by the polaron hopping conduction. In the future, we will incorporate the ferroelectric domain structure and study the coupling behaviors between space charges and polarization to understand their effect on the resistance degradation in ferroelectric capacitors. ACKNOWLEDGMENTS The authors are grateful to the financial support for NSF-IUCRC Center for Dielectric Studies at Penn State. The work of Jie Shen is partially supported by NSF DMS- 1215066 and by the Computational Materials and Chemical Sciences Network (CMCSN) APPENDIX: CHEBYSHEV COLLOCATION ALGORITHM We introduced the Chebyshev collocation method to solve the second-order partial differential equation FIG. 7. Calculated leakage current evolution considering the small polaron hopping conduction mechanism under 1.0 V dc bias at 150 /C14 C. FIG. 8. Calculated polaron concentration in cathode vs. leakage current den- sity in the resistance degradation process (from 5 to 40 s with 5 s interval). FIG. 6. Evolution of polaron under flux boundary condition in SrTiO 3 under 1.0 V dc bias. 224102-6 Cao et al. J. Appl. Phys. 114, 224102 (2013) [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27 eu00ðxÞþ pðxÞu0ðxÞþ qðxÞuðxÞ¼ f ðxÞ in ð/C0 1; 1Þ2; (A1) where e is a fixed parameter and pðxÞ, qðxÞ,a n d f ðxÞ are the given functions. The boundary condition for Eq. (A1) is given by a/C0 u /C0 1ðÞ þ b/C0 u0 /C0 1ðÞ ¼ c/C0 ; aþu þ1ðÞ þ bþu0 þ1ðÞ ¼ cþ: (A2) We first consider the Dirichlet boundary condition uð/C0 1Þ¼ c/C0 ; uðþ1Þ¼ cþ: (A3) The Chebyshev interpolation polynominal can be written as uN ðxÞ¼ Xn j¼1 UjFjðxÞ; (A4) where xj ¼ cos jp=NðÞ ,0 /C20 j /C20 N are the Chebyshev-Gauss- Lobatto collocation points, Uj are the unknown coefficients to be determined, and FjðxÞ is the Lagrange interpolation polynominal associated with xjfg . The Chebyshev colloca- tion method is to seek uN in the form of Eq. (A4) such that uN ð/C0 1Þ¼ c/C0 , uN ðþ1Þ¼ cþ and Eq. (18) holds at the inte- rior collocation points euN xxðxjÞþ pðxjÞuN x ðxjÞþ qðxjÞuN ðxjÞ¼ f ðxjÞ; i /C20 j /C20 N /C0 1: (A5) By using the definition of the differentiation matrix (details can be found in Ref. 15), we obtain a set of linear equations XN/C0 1 j¼1 eðD2Þij þ pðxiÞðD1Þij þ qðxiÞdij hi Uj ¼ f ðxiÞ/C0 eðD2Þi0 þ pðxiÞðD1Þi0 /C2/C3 cþ /C0 eðD2ÞiN þ pðxiÞðD1ÞiN /C2/C3 c/C0 ; (A6) for the Ujfg N/C0 1 j¼1 ,i nw h i c hdij is the Kronecker delta. To sum- marize, the spectral-collocation solution for Eq. (A1) with Dirichlet boundary conditions Eq. (A3) satisfies the linear system A /C22U ¼ /C22b; (A7) where /C22U ¼ U1; :::; UN/C0 1½/C138 T , the matrix A ¼ aijðÞ , and the vector /C22b are given by aij ¼ eðD2Þij þ pðxiÞðD1Þij þ qðxiÞdij; 1 /C20 i; j /C20 N /C0 1; bi ¼ f ðxiÞ/C0 eðD2Þi0 þ pðxiÞðD1Þi0 /C2/C3 cþ /C0 eðD2ÞiN þ pðxiÞðD1ÞiN /C2/C3 c/C0 ; 1 /C20 i /C20 N /C0 1: (A8) The solution to the above system gives the approximate solu- tion to Eqs. (A1) and (A3) at the collocation points. For gen- eral boundary conditions, the procedure is similar. The details of the solution can be found in Ref. 18. 1O. Auciello, J. F. Scott, and R. Ramesh, Phys. Today 51(7), 22 (1998). 2W. Liu and C. A. Randall, J. Am. Ceram. Soc. 91, 3245 (2008). 3W. Liu and C. A. Randall, J. Am. Ceram. Soc. 91, 3251 (2008). 4H. I. Yoo, M. W. Chang, T. S. Oh, C. E. Lee, and K. D. Becker, J. Appl. Phys. 102, 093701 (2007). 5R. Waser, T. Baiatu, and K. H. Hardtl, J. Am. Ceram. Soc. 73, 1654 (1990). 6G. Y. Yang, G. D. Lian, E. C. Dickey, C. A. Randall, D. E. Barber, P. Pinceloup, M. A. Henderson, R. A. Hill, J. J. Beeson, and D. J. Skamser, J. Appl. Phys. 96, 7500 (2004). 7S. H. Yoon, C. A. Randall, and K. H. Hur, J. Am. Ceram. Soc. 92, 2944 (2009). 8S. H. Yoon, S. H. Kwon, and K. H. Hur, J. Appl. Phys. 109, 084117 (2011). 9T. Baiatu, R. Waser, and K. H. Hardtl, J. Am. Ceram. Soc. 73, 1663 (1990). 10T. Holbling, N. Soylemezoglu, and R. Waser, J. Electroceram. 9,8 9 (2002). 11R. Meyer, R. Liedtke, and R. Waser, Appl. Phys. Lett. 86, 112904 (2005). 12C. A. Randall, R. Maier, W. Qu, K. Kobayashi, K. Morita, Y. Mizuno, N. Inoue, and T. Oguni, J. Appl. Phys. 113, 014101 (2013). 13D. B. Strukov, J. L. Borghetti, and R. S. Williams, Small 5, 1058 (2009). 14W. Liu, G. Y. Yang, and C. A. Randall, Jpn. J. Appl. Phys., Part 1 48, 051404 (2009). 15L. Q. Chen and J. Shen, Comp. Phys. Commun. 108, 147 (1998). 16T. Okamoto, S. Kitagawa, N. Inoue, and A. Ando, Appl. Phys. Lett. 98, 072905 (2011). 17S. Zhao, S. J. Zhang, W. Liu, N. J. Donnelly, Z. Xu, and C. A. Randall, J. Appl. Phys. 105, 053705 (2009). 18J. Shen and T. Tang, Spectral and High-Order Methods with Applications (Science Press, Beijing, China, 2006). 224102-7 Cao et al. J. Appl. Phys. 114, 224102 (2013) [This article is copyrighted as indicated in the article. Reuse of AIP content is subject to the terms at: http://scitation.aip.org/termsconditions. Downloaded to ] IP: 128.210.4.213 On: Fri, 14 Mar 2014 13:47:27

采集于

查看校方原文 ↗