校园网页 · 学校官网
Effect of multi-domain structure on ionic transport, electrostatics, and current evolution in BaTiO3 ferroelectric capacitor
Full length article Effect of multi-domain structure on ionic transport, electrostatics, and current evolution in BaTiO 3 ferroelectric capacitor Ye Cao a, *, Jie Shen b, Clive Randall a, Long-Qing Chen a a Department of Materials Science and Engineering, The Pennsylvania State University, University Park, PA 16802, USA b Department of Mathematics, Purdue University, W Lafayette, IN 47907, USA article info Article history: Received 1 1 January 2016 Accepted 9 April 2016 Keywords: Defect transport BaTiO 3 Domain structure Resistance degradation Phase-field simulation abstract The semiconducting properties of certain ferroelectric materials, partially caused by the interactions among ferroelectric polarizations, charged domain walls, and conducting point defects, pose a threat to the reliability of ferroelectrics used as dielectric material in capacitor devices, and is not yet fully un- derstood. We proposed a physical model combining the phase- field method for ferroelectric domain structures and diffusion equations for defect transport to study the resistance degradation behavior in multi-domain tetragonal BaTiO 3 capacitors. We considered a hypothetical Ni/BaTiO 3/Ni single parallel plate capacitor con figuration subject to 0.5 V dc bias at 25 /C14 C. It is found that 90 /C14 domain walls are charged, induce local space charge segregation, and form local electric potential barriers upon external bias that signi ficantly influence the ionic transport behavior. Additionally, the 180 /C14 domain walls remain nearly charge neutral and have much less in fluence on ionic transport. The effect of domain wall and polarization orientations on the leakage current evolution is investigated. Our study could necessitate further understanding on the in fluence of ferroelectric state, ionic interactions, transport barriers, spatial distributions, and breakdown phenomena. © 2016 Acta Materialia Inc. Published by Elsevier Ltd. All rights reserved.1. Introduction Ferroelectric oxides, such as barium titanite (BaTiO 3), have been extensively used as dielectric materials in multi-layer ceramic ca- pacitors (MLCCs) in various electronic devices [1]. The trend of further miniaturization of MLCC devices for high capacitance resulted in ever-decreasing dielectric thickness, down to sub- micron levels, and ever-increasing electric field strength distrib- uted across each dielectric layer under given voltage stresses [2]. This causes a major challenge to the reliability of MLCCs, among which the long-term resistance degradation is one of the primary limiting factors to the life time of MLCCs. The long-term resistance degradation is characterized by slowly increasing leakage currents under a DC bias well below the critical breakdown voltage [3]. In the dielectric industry, the evaluations of resistance degra- dation, and thus the long-term reliability of MLCCs, are generally accessed by an engineering approach called the highly accelerated lifetime tests (HALTs) [3,4]. This method evaluates the lifetime of MLCCs by extrapolating the HALTs data measured under various temperatures and field stresses to the real working condition based on the Erying model [5]. Although this method shows advantages in accelerating the measurement at high temperature and voltage stress in paraelectric phase, it rules out the possible in fluence of complex ferroelectric domain structures and the associated piezoelectric strains on the degradation process of ferroelectric- based capacitor. Therefore, the HALTs evaluated long-term reli- ability accessed in the paraelectric phase may not represent the real lifetime of ferroelectric capacitors. On the other hand, it is of scienti fic importance to understand the mechanism of the ion transport and its relationship to resis- tance degradation. Over the past 20 years, it has been investigated by a number of experimental approaches, including the electro- coloration measurement [6,7], impedance spectroscopy (IS) [8], thermal simulated depolarization current (TSDC) [9,10], trans- mission electron microscopy (TEM) [1 1], and theoretical calcula- tions, such as finite element method [12e14]. While it is generally recognized that the oxygen vacancy migration plays an important role in the degradation process, it is still unclear how the ferro- electric domain structures could in fluence the ionic/electronic distribution and transport behavior. The authors have recently studied the effect of ferroelectric polarization on resistance * Corresponding author. E-mail address: yxc238@psu.edu (Y. Cao). Contents lists available at ScienceDirect Acta Materialia journal homepage: www.elsevier.com/l ocate/actamat http://dx.doi.org/10.1016/j.actamat.2016.04.027 1359-6454/© 2016 Acta Materialia Inc. Published by Elsevier Ltd. All rights reserved. Acta Materialia 1 12 (2016) 224e230 degradation behavior in single domain BaTiO 3 capacitor [15]; however, a single domain con figuration is rarely formed in real BaTiO3 capacitors. It was reported that domain walls contribute to the dielectric and piezoelectric properties of ferroelectric materials [16,17]and could pin the local space charge and affect the transport behavior due to the polarization charges [18e21] and mechanical stresses [22,23] developed along ferroelastic domain walls. There- fore, to obtain a more complete fundamental understanding of resistance degradation behavior in ferroelectric capacitor, a physics-based theoretical model capable of incorporating the multi-domain structure and defect transport interaction is imperative. In this work, we developed a combined phase- field and trans- port model to understand the role of ferroelectric domain and domain walls on ionic transport and resistance degradation behavior, and to estimate the long-term reliability of real ferro- electric based capacitor. The phase- field method has been suc- cessfully applied to studying the ferroelectric domain structures in both bulk and thin film systems [24e28]. In this study, we chose the sandwiched Ni/BaTiO3/Ni single parallel plate capacitor con figura- tion as the model system. The effects of ferroelectric/metal in- terfaces and domain wall orientations on the ionic segregation/ depletion, local electric potential and field distribution, and ionic migration upon external field and leakage current evolution have been extensively studied. Our work provides some fundamental insights into the complex interactions among ferroelectric domain structure, defect transport and dielectric degradation behavior. 2. Model In the phase- field model of multi-domain BaTiO 3 capacitor, the ferroelectric system is represented by choosing the polarization vector Pi ¼ (P1,P2,P3) as the order parameter to describe the ferro- electric domain structures. The domain evolution is modeled by the temporal evolution of Pi obtained by minimizing the total free en- ergy of the system with respect to Pi, vPiðr; tÞ vt ¼/C0 L dF dPiðr; tÞ; ði ¼ 1 /C24 3Þ (1) in which t is the time step and L is the kinetic coef ficient related to domain mobility. The total free energy F of BaTiO3 single crystal is expressed as, F ¼ Z V h flanðPiÞþ fgrad /C0 Pi;j /C1 þ felas /C0 Pi; εij /C1 þ felecðPi; EiÞ i dV (2) where V is the system volume, εij and Ei denote the components of strain and electric field, Pi,j ¼ vPi/xj, and flan(Pi), fgrad(Pi,j), felas(Pi,εij) and felec(Pi,Ei) represent the Landau-Devonshire free energy den- sity, the gradient energy density, and elastic energy density and the electrostatic energy density, respectively. Detailed expressions of each of the local free energy densities can be found in literature [25,26]. The charge defect distribution, transport, and blocking at elec- trodes play an important role in resistance degradation phenom- ena. In this study, the intrinsic and extrinsic major charge defects of interest include the oxygen vacancies (V $$ O ), electrons (e 0 ), holes (h/C15 ), and ionized acceptors ( A 0 ) written in Kr €oger-Vink notation [29]. The þ2 oxygen vacancies are created during high temperature annealing of capacitors, and their concentration is assumed to be conserved at the temperature when degradation measurements are conducted. The acceptors are introduced by substitution of þ3 el- ements, such as Fe and Al, on the þ4 Ti sites (Fe0 Ti and Al0 Ti ¼ A0) and are considered fully ionized and immobile. We assumed in the simulation that all the charged carriers are homogeneously distributed in the entire BaTiO 3 layer, and local charge neutrality condition is satis fied in the initial state, rðxÞ¼ X i zie0ciðxÞ¼ 0 /C0 i ¼ V$$ O ; p; n; A0/C1 (3) where r(x) is the space charges at positon x, e0 is the unite charge, ci and zi are the concentration and charge number of given species i. (zV$$ O ¼þ 2,zh$ ¼þ 1 and ze0 ¼ zA0 ¼/C0 1) The migrations of the mo- bile charge defects are described by solving the linear transport equations, considering only concentration gradient and local elec- tric field as the driving forces, J . i ¼/C0 Di V . ci þ zimici E .vci vt ¼/C0 V . $ J . i (4) in which Ji,Di,mi denote the flux, diffusivity, and mobility of given charge species i. V . ¼ v vx i . þ v vy j . þ v vz k . is the gradient operator. E . is the local electric field component. We assume that the plate electrodes form blocking contact to the oxygen vacancy transport, thus the boundary condition of Eq. (4) for oxygen vacancy is specified as, J . V$$ O ¼ 0 (5) On the other hand, the mobility of electrons and holes are several orders of magnitude higher than that of oxygen vacancy. They are assumed to reach steady state for each oxygen vacancy evolution. Mathematically we solve the steady state equations for electron ( vn/vt ¼ 0) and hole evolution ( vp/vt ¼ 0). The electronic concentrations at the metal/ferroelectric interfaces are fixed by the work function of the metal electrode (Ni). The boundary conditions of Eq. (4) for electrons and holes are written as, nz¼0:L ¼ Nc exp /C18 /C0 Ec /C0 Efm kBT /C19 pz¼0:L ¼ Nv exp /C18 /C0 Efm /C0 Ev kBT /C19 (6) in which Nc and Nv are the effective density of states in the con- duction and valence band of BaTiO 3, where Ec and Ev represent the energy of the conduction band minimum and valence band maximum. Efm is the work function of plate electrode, and kB is the Boltzmann constant. The interaction between electric potential, space charge, and polarization induced bound charge are described by the electro- static equilibrium equation considering the space charge distribution, Di;i ¼ D1;1 þ D2;2 þ D3;3 ¼ r (7) in which Di,i ¼ vDi/vxi while Di is the electric displacement, which is related to the electric field and polarization component through, Di ¼ k0kijEj þ Piði ¼ 1 /C24 3Þ (8) in which k0 is the vacuum permittivity and kij is the dielectric constant. The polarization induced charges are introduced by /C0 Pi,i ¼/C0 (P1,1 þ P2,2 þ P3,3), and the electric field E . is related to the electric potential through, Ei ¼/C0 f;iði ¼ 1 /C24 3Þ (9) Combining Eqs. (7)e(9) and assuming kij ¼ 0(isj), the Y. Cao et al. / Acta Materialia 1 12 (2016) 224 e230 225 electrostatic equilibrium equation (Eq. (7)) can be rewritten as, k11f;11 þ k22f;22 þ k33f;33 ¼ 1 k0 /C0 P1;1 þ P2;2 þ P3;3 /C0 r /C1 (10) The boundary condition for Eq. (10) is defined as, fjz¼0 ¼ Vað0Þ; fjz¼L ¼ VaðLÞ (11) in which Va(0) and Va(L) are speci fied from the externally applied potential bias at z ¼ 0,L. To model the polarization induced bound charges at the Ni/ BaTiO3 interfaces, we specify the polarization distribution at the boundaries as, a/C2 Pi /C0 b /C2 dPi dz /C12/C12/C12 /C12 z¼0 ¼ 0; a/C2 Pi þ b /C2 dPi dz /C12/C12/C12 /C12 z¼L ¼ 0ði ¼ 1 /C24 3Þ (12) where the coef ficients a and b are chosen to be 1.0 and 0.05 cm to represent the case where the charges at the metal/ferroelectric interfaces are partially compensated. The current density is contributed from the flow of mobile charged defects, including oxygen vacancies, electrons, and holes. The current density for particular charged carrier i and the total current density are given by, Ii ¼ zie0Ji Itotal ¼ X i Ii (13) where i only include mobile species ( i ¼ V·· O; e0; h$). 3. Simulation results and discussion 3.1. Initial setup We started with a preset 2D multi-domain tetragonal BaTiO 3 as the model system, which consists of four possible domain variants, i.e., aþ(100), a/C0 (/C0 100), cþ(001), and ce(00e1) in a head-to-tail configuration to form both 180 /C14 and 90 /C14 domain walls ( Fig. 1(a)). The BaTiO 3 film is 500 nm in thickness and is constrained by Ni plate electrodes of normal vector along z (001). The external applied bias is along þ z direction. We set up a coordinate system Fig. 1. 2D plot of the equilibrium state of (a) domain structure, (b) polarization induced bound charges ( i ¼ 1e3), (c) oxygen vacancy distribution, (d) electric potential distribution and (e) shear stress s5. (f) 1D comparison of space charge (solid lines) and polarization charge (dashed lines) distributions along particular directions as indicated by t he red and green dashed lines in (a). The red and green ordinates in (f) (note with different scales) are for charge distributions along direction (1) and (2) resp ectively as indicated in (a). (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) Table 1 Parameters used in the simulation. Parameter Value Parameter Value Temperature, T (K) 298 Conduction band, Ec (eV) [19] /C0 3.6 Total thickness, L (nm) 500 Valence band, Ev (eV) /C0 6.7 External applied bias (V) 0.5 Work function of Ni electrode, Efm (eV) /C0 5.2 Oxygen vacancy mobility, mV$$ O (cm2$V/C0 1$s/C0 1 ) [7] 1.0 /C2 10/C0 14 Effective Density of States, Nc, Nv (cm/C0 3) [12] 1022 Y. Cao et al. / Acta Materialia 1 12 (2016) 224 e230226 with periodic boundary condition along x (100) direction and non- periodic general boundary condition along z (001) direction. The simulation size is discretized into a 2D mesh of 400 Dx /C2 400Dz, while Dz is non-uniform. The temporal evolution of the polariza- tions and defect concentrations are obtained by solving the time- dependent Ginzburg-Laudau (TDGL) equations (Eqs (1)) and transport equations (Eqs (4)) using the combined semi-implicit Fourier spectral method [30] and Chebyshev collocation method [31]. The material constants and energy coef ficients are taken from the literature [28]. The parameters used in the simulation are listed in Table 1. 3.2. Equilibrium state We first evolved the preset domain structure under room tem- perature without an external bias (U DC ¼ 0) to reach equilibrium state, in which both 90 /C14 and 180/C14 domain walls become stable and form a step-like domain con figuration ( Fig. 1(a)). It is clearly seen that the positive/negative alternating polarization charges are bounded to the 90/C14 domain walls, while the 180/C14 domain walls and the domain interior remain charge neutral ( Fig. 1(b)). This is due to the gradual rotations of polarizations across 90 /C14 domain walls of finite thickness. The 90 /C14 charged domain walls are locally compensated by an ionic (oxygen vacancy) segregation (Fig. 1(c)). It should be noted that the electronic charge compensation is negli- gible, since electronic charges are assumed to be fixed at the metal/ ferroelectric interfaces in the simulation, and consequently their concentrations are much lower than ionic charge carriers. The ionic charges do not fully compensate the polarization bound charges. This induces a small internal electric potential even in the absence of external applied bias ( Fig. 1(d)), and a negative shear stress ( s5) along the 90 /C14 domain walls ( Fig 1 (e)). A 1-D plot of the charge distributions along particular directions (indicated by red and green dashed lines in (a)) clearly shows that only 90 /C14 domain walls exhibit alternating polarization charges (dashed lines in (f)) and space charges (solid lines in (f)) (always in the opposite direction for compensation), with the latter being much smaller than the former in magnitude. The resulting net charges are between /C0 5.0e5.0 C/cm 3 across the 90 /C14 domain walls. Notably large polarization charges are also found at the metal/ferroelectric interfaces, where the polarizations are oriented perpendicular to the contacting plate electrodes (green dashed lines in (f), not shown in (b)). This is because the electrodes are assumed to partially compensate the polarization charges. When the polarizations are oriented parallel to the contacting electrodes, there are no inter- facial charges induced (pink dashed lines in (f)). 3.3. Evolution under applied bias When the domain structure and the local charges reach an equilibrium state, a dc bias of 0.5 V is applied along þ z direction. Fig. 2 (a)e(d) show the temporal evolution of oxygen vacancies along z directions across the center of each of the 1/4 sections of the entire domain (the corresponding domain structures are shown in Fig. 2. 1D plot of oxygen vacancy evolution along z direction in each of the 1/4 of the entire multi-domain BaTiO 3 under UDC ¼ 0.5 V at room temperature: (a) x/H ¼ 0.0e0.5; (b) x/ H ¼ 0.5e1.0; (c) x/H ¼ 1.0e1.5; (d) x/H ¼ 1.5e2.0. (H ¼ 250 nm is half of the film thickness, so that z/H from /C0 1t o þ1 represents the entire film thickness). Y. Cao et al. / Acta Materialia 1 12 (2016) 224 e230 227 the insets). Under the applied bias, oxygen vacancies electro- migrate towards the cathode side ( z/H ¼ 1.0), which results in ionic segregation in the vicinity of the cathode region and depletion in the anode region (z/H ¼/C0 1.0). It is also seen that part of the oxygen vacancies pile up in front of the 90 /C14 domain walls and under these conditions are locally trapped and not free to migrate towards cathode, due to the polarization charges along 90 /C14 domain walls. This becomes obvious in those domains with local polarizations oriented along the transport direction ( þz), where ionic enrich- ment and depletion are both seen locally inside the domain. Such local ionic redistribution are also seen in domains of polarization orientation opposite to the transport direction ( /C0 z), but the extent of local enrichment/depletion is less than the previous case. On the other hand, 180 /C14 domain walls are less, if not at all, charged and have nearly no in fluence on the oxygen vacancy transport. Clearly, the polarizations along þ z directions tend to promote the oxygen vacancy transport, as is further evidenced by the maximum local oxygen vacancy accumulation of ~10 20 cm/C0 3 found at the cathode region, where adjacent domain is along þ z (Fig. 2 (c)) and agrees with previous report [15]. To further understand the interaction between the 90 /C14 domain walls and ionic transport, we studied the electric potential and field distribution under U DC ¼ 0.5 V. Fig. 3 (a)e(d) show the 1D electric potential (solid black lines) and electric field (solid red lines) dis- tributions across the center of each of the 1/4 sections of the entire domain at time t ¼ 2.5 /C2 106s. The light blue arrows represent the domain orientations along z directions, while the dashed lines indicate the domain wall positions. From Fig. 3 , the electric po- tential drops are mainly seen in “/” oriented domains along the applied field direction. This also explains why oxygen vacancy transports are promoted in those local domains (Fig. 2). The electric potential drops become much smaller in domains with “)”, “Y” and “[”orientations that are not adjacent to the electrodes. On the other hand, remarkable electric potential gradients and local elec- tric field enhancements can be found across the 90 /C14 domain walls (indicated by red and green dashed lines). For “Y\)” and “)\Y” types of domain walls (indicated by green dashed lines), the drops of electric potential induce local positive electric fields of ~þ100 kV/ cm. The oxygen vacancy drift under this positive field counterbal- ances oxygen vacancy diffusion in the opposite direction due to the local concentration gradient, which is induced by the polarization charges located at the 90/C14 domain wall. This is further illustrated by a combined replot of Figs. 1(f), 2(b) and 3(b) into Fig. 4. For “[\/” and “/\[” types of domain walls (indicated by red dashed lines), local potential barriers are formed with negative local electric fields to block the ionic transport. This causes local ionic accumulation and depletion on each side of the 90 /C14 domain walls. The 180 /C14 domain walls (indicated by blue dashed lines in Fig. 3 ) are less interacted with the electric potential distributions, and the electric fields are much smaller than those found at 90 /C14 domain walls. 3.4. In fluence of domain structure on leakage current evolutions The effects of multi-domain structures on leakage current Fig. 3. 1D plot of electric potential (black solid lines) and electric field (red solid lines) distributions at t ¼ 2.5 /C2 106s along z direction in each of the 1/4 of the entire multi-domain BaTiO3 under UDC ¼ 0.5 V at room temperature: (a) x/H ¼ 0.0e0.5; (b) x/H ¼ 0.5e1.0; (c) x/H ¼ 1.0e1.5; (d) x/H ¼ 1.5e2.0. The light blue arrows indicate the domain orientations. Dark blue dashed lines indicate the positions of 180 /C14 domain walls, green dashed lines indicate the positions of 90 /C14 domain walls (Y\)\Y) where electric potential locally drops, and red dashed lines indicate the positions of 90 /C14 domain walls ([\/\[) where there is local electric potential barrier blocking the ionic transport. (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) Y. Cao et al. / Acta Materialia 1 12 (2016) 224 e230228 evolution in Ni/BaTiO 3/Ni single layer capacitor under DC bias are further investigated. For comparison, we considered four additional scenarios of BaTiO 3 composed of: (1) single domain of P z along þ z direction (along the applied field direction), (2) single domain of P z along -z direction, (3) 90 /C14 domain structure composed of “[\/” and “/\[” types of domain walls, and (4) 90 /C14 domain structure composed of “Y\)” and “)\Y” types of domain walls. They are schematically illustrated in Fig. 5 (a), and the current density evo- lutions for scenario (1) e(4) and multi-domain structure (5) are plotted and compared in Fig. 5 (b). It is seen that the leakage cur- rents increase slowly in the initial steps, followed by a fast and significant increase, which indicates the dielectric breakdown of capacitors. The sudden increases of leakage currents are attributed to the oxygen vacancy migrations and accumulations at the cathode regions. By comparing the degradation characteristic time ( tch), which is defined as the critical time when leakage current increases 10 /C2 compared to its initial value (marked by “þ” in Fig 5(b)), it is found that tch is fastest in single cþ domain ( tch ~ 4.6 /C2 105s, sce- nario (1)) and slowest in single c-domain ( tch > 2 /C2 106s, scenario (2)). Clearly, the polarization accelerates the degradation process when it is in the field direction ( þz). Similarly the leakage currents in “[\/\[” type of 90 /C14 domain structure ( tch ~7 . 7/C2 105s, scenario (3)) increase faster than in “Y\)\Y” type of 90 /C14 domain structure (tch~1.28 /C2 106s, scenario (4)). This is because the trend of the po- larization direction is still along the applied field direction in (3) and reverses to the field direction in (4). Notably, tch in (3) is also slower than that in (1), since domain structure of (3) consists of half aþ and cþ domain types, with only cþ contributing to the current evolution and the rest aþ less interacted with the ionic transport. The charged 90 /C14 domain walls in (3) could also impede the oxygen vacancy migration and, consequently, the leakage current increase. Conversely, the current increases faster in (4) compared to (2), since the former structure consists of only half c-domain that is known to inhibit current increase. Finally, the multi-domain structure is considered a combination of all possible a/c domains and 180/C14 /90/C14 domain walls; therefore, the tch is expected to be average of the other four scenarios ( tch ~ 9.4 /C2 105 s). 4. Conclusions In this work, we developed a phase- field model combined with transport equations to study the space charge distribution, ionic transport, electrostatic evolution, and resistance degradation of a preset multi-domain structure BaTiO 3 single plate ferroelectric capacitor. Our results show that polarization induced bound charges along 90 /C14 domain walls account for the local oxygen va- cancy segregation, while the 180 /C14 domain walls and domain in- teriors remain charge neutral and have less in fluence on the defect distribution. Upon an external DC bias, remarkable electric Fig. 4. Illustration of interactions between polarization charges, ionic transport, and electric potential/ field by replotting Figs. 1(f), 2(b) and 3(b) into Fig. 4 (a)e(c). The electric potential drop at the 90 /C14 domain wall (green dashed lines) induces local positive electric field to facilitate the oxygen vacancy drift (c), and counterbalances the oxygen vacancy diffusion in the opposite direction due to local concentration gradient (b), which is induced by the positive/negative polarization charges aside the 90 /C14 domain wall (a). (For interpretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) Fig. 5. (a) Schematic plot of possible domain con figurations of BaTiO 3 and (b) com- parison of current density evolution of BaTiO 3 capacitor of different domain con figu- rations at 25 /C14 C under U DC ¼ 0.5 V. The colors of the schematic domain con figurations in (a) correspond to the colors of the current density evolution in (b). The “þ” mark the degradation characteristic time ( tch) for different domain con figurations. (For inter- pretation of the references to colour in this figure legend, the reader is referred to the web version of this article.) Y. Cao et al. / Acta Materialia 1 12 (2016) 224 e230 229 potential gradient and potential barrier, and the resulting local electric field concentration, are observable at the 90 /C14 charged domain walls, which partially blocks the oxygen vacancies migra- tion, resulting in a local ionic enrichment and depletion on either side of the 90 /C14 domain walls. On the other hand, the effect of 180 /C14 domain walls on local electrostatics and oxygen vacancy evolution is hardly seen. The in fluence of multi-domain structure on the resistance degradation behavior under room temperature is further investigated by comparing the leakage current evolutions and degradation characteristic time ( t ch) among different possible domain configurations in BaTiO 3. Acknowledgements The work at Penn State was supported by U.S. Department of Defense, Air Force under FA9550-14-1-0264 (Chen) and FA9550- 14-1-0067 (Randall), and the National Science Foundation as part of the IUCRC Center for Dielectrics and Piezoelectrics under Grant No. IIP-1361571 at Penn State. The work of Shen is partially supported by NSF DMS-1215066 and by the Computational Materials and Chemical Sciences Network (CMCSN). References [1] H. Kishi, Y. Mizuno, H. Chazono, Base-metal electrode-multilayer ceramic capacitors: past, present and future perspectives, Jpn. J. Appl. Phys. 1 (42) (2003) 1 e15. [2] A.V. Polotai, A.V. Ragulya, C.A. Randall, Preparation and size effect in pure nanocrystalline barium titanate ceramics, Ferroelectrics 288 (2003) 93 e102. [3] R. Waser, T. Baiatu, K.H. Hardtl, Dc electrical degradation of perovskite-type titanates .1. Ceramics, J. Am. Ceram. Soc. 73 (1990) 1645 e1653. [4] S. Zhao, S.J. Zhang, W. Liu, N.J. Donnelly, Z. Xu, C.A. Randall, Time dependent dc resistance degradation in lead-based perovskites: 0.7 Pb(Mg 1/3Nb2/3)O3-0.3 PbTiO3, J. Appl. Phys. 105 (2009) 053705 . [5] C.A. Randall, R. Maier, W. Qu, K. Kobayashi, K. Morita, Y. Mizuno, N. Inoue, T. Oguni, Improved reliability predictions in high permittivity dielectric oxide capacitors under high dc electric fields with oxygen vacancy induced elec- tromigration, J. Appl. Phys. 113 (2013) 014101 . [6] R. Waser, T. Baiatu, K.H. Hardtl, Dc electrical degradation of perovskite-type titanates .2. Single-Crystals, J. Am. Ceram. Soc. 73 (1990) 1654 e1662. [7] H.I. Yoo, M.W. Chang, T.S. Oh, C.E. Lee, K.D. Becker, Electrocoloration and oxygen vacancy mobility of BaTiO 3, J. Appl. Phys. 102 (2007) 093701 . [8] W. Liu, G.Y. Yang, C.A. Randall, Evidence for increased polaron conduction near the cathodic interface in the final stages of electrical degradation in SrTiO3 crystals, Jpn. J. Appl. Phys. 48 (2009) 051404 . [9] W. Liu, C.A. Randall, Thermally stimulated relaxation in Fe-Doped SrTiO 3 systems: I. Single crystals, J. Am. Ceram. Soc. 91 (2008) 3245 e3250. [10] W. Liu, C.A. Randall, Thermally stimulated relaxation in Fe-Doped SrTiO3 Systems: II. Degradation of SrTiO 3 dielectrics, J. Am. Ceram. Soc. 91 (2008) 3251e3257. [11] G.Y. Yang, G.D. Lian, E.C. Dickey, C.A. Randall, D.E. Barber, P. Pinceloup, M.A. Henderson, R.A. Hill, J.J. Beeson, D.J. Skamser, Oxygen nonstoichiometry and dielectric evolution of BaTiO 3. Part II - insulation resistance degradation under applied dc bias, J. Appl. Phys. 96 (2004) 7500 e7508. [12] T. Baiatu, R. Waser, K.H. Hardtl, Dc electrical degradation of perovskite-type titanates .3. A model of the mechanism, J. Am. Ceram. Soc. 73 (1990) 1663e1673. [13] T. Holbling, N. Soylemezoglu, R. Waser, A mathematical-physical model for the charge transport in p-type SrTiO 3 ceramics under dc load: maxwell- Wagner relaxation, J. Electroceramics 9 (2002) 89 e102. [14] R. Meyer, R. Liedtke, R. Waser, Oxygen vacancy migration and time- dependent leakage current behavior of Ba 0.3Sr0.7TiO3 thin films, Appl. Phys. Lett. 86 (2005) 112904 . [15] Y. Cao, J. Shen, C. Randall, L.Q. Chen, Effect of ferroelectric polarization on ionic transport and resistance degradation in BaTiO 3 by Phase-field approach, J. Am. Ceram. Soc. 97 (2014) 3568 e3575. [16] D. Damjanovic, Ferroelectric, dielectric and piezoelectric properties of ferro- electric thin films and ceramics, Rep. Prog. Phys. 61 (1998) 1267 e1324. [17] D. Damjanovic, Stress and frequency dependence of the direct piezoelectric effect in ferroelectric ceramics, J. Appl. Phys. 82 (1997) 1788 e1797. [18] Y. Xiao, K. Bhattacharya, Interaction of oxygen vacancies with domain walls and its impact on fatigue in ferroelectric thin films, in: Smart Structures and Materials 2004: Active Materials: Behavior and Mechanics 5387, 2004, pp. 354e365. [19] Y. Xiao, V.B. Shenoy, K. Bhattacharya, Depletion layers and domain walls in semiconducting ferroelectric thin films, Phys. Rev. Lett. 95 (2005) 247603 . [20] Q.S. Zhang, W.A. Goddard, Charge and polarization distributions at the 90 degrees domain wall in barium titanate ferroelectric, Appl. Phys. Lett. 89 (2006) 182903 . [21] J. Hlinka, P. Marton, Phenomenological model of a 90 degrees domain wall in BaTiO3-type ferroelectrics, Phys. Rev. B 74 (2006) 104104 . [22] C. Korte, N. Schichtel, D. Hesse, J. Janek, In fluence of interface structure on mass transport in phase boundaries between different ionic materials Experimental studies and formal considerations, Monatsh Chem. 140 (2009) 1069e1080. [23] N. Schichtel, C. Korte, D. Hesse, J. Janek, Elastic strain at interfaces and its influence on ionic conductivity in nanoscaled solid electrolyte thin films- theoretical considerations and experimental studies, Phys. Chem. Chem. Phys. 11 (2009) 3043 e3048. [24] H.L. Hu, L.Q. Chen, Computer simulation of 90 degrees ferroelectric domain formation in two-dimensions, Mater. Sci. Eng. A Struct. Mater. Prop. Micro- struct. Process. 238 (1997) 182 e191. [25] Y.L. Li, S.Y. Hu, Z.K. Liu, L.Q. Chen, Phase- field model of domain structures in ferroelectric thin films, Appl. Phys. Lett. 78 (2001) 3878 e3880. [26] Y.L. Li, S.Y. Hu, Z.K. Liu, L.Q. Chen, Effect of substrate constraint on the stability and evolution of ferroelectric domain structures in thin films, Acta Mater 50 (2002) 395 e411. [27] Y.L. Li, L.Q. Chen, G. Asayama, D.G. Schlom, M.A. Zurbuchen, S.K. Streiffer, Ferroelectric domain structures in SrBi 2Nb2O9 epitaxial thin films: electron microscopy and phase- field simulations, J. Appl. Phys. 95 (2004) 6332 e6340. [28] Y.L. Li, L.E. Cross, L.Q. Chen, A phenomenological thermodynamic potential for BaTiO3 single crystals, J. Appl. Phys. 98 (2005) 064101 . [29] F.A. Kroger, H.J. Vink, Relations between the concentrations of imperfections in crystalline solids, Solid State Phys. 3 (1956) 307 e435. [30] L.Q. Chen, J. Shen, Applications of semi-implicit Fourier-spectral method to phase field equations, Comput. Phys. Commun. 108 (1998) 147 e158. [31] Y. Cao, S. Bhattacharya, J. Shen, C.A. Randall, L.Q. Chen, Role of polaron hop- ping in leakage current behavior of a SrTiO 3 single crystal, J. Appl. Phys. 114 (2013) 224102 . Y. Cao et al. / Acta Materialia 1 12 (2016) 224 e230230
采集于
查看校方原文 ↗